Catalysis of Metal-Acid Reaction: Copper(II) on Zinc and Acid

Show that traces of copper(II) ions catalyse the reaction between zinc and sulfuric acid.

Level: UniversitySafety: SafeTime: 45 min
Aim of Experiment: Show that traces of copper(II) ions catalyse the reaction between zinc and sulfuric acid.

Theoretical Foundations

Zn + H2SO4 -> ZnSO4 + H2 is slow with pure zinc, but Cu2+ plates copper onto the zinc, forming a Zn-Cu galvanic couple that greatly accelerates electron transfer. The Cu2+ is regenerated in the cycle, acting as a catalyst.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Test tubes
  • Stopwatch
  • Balance
  • Measuring cylinders

Chemical Reagents

  • Zinc granules
  • Sulfuric acid, 1.0 M
  • Copper(II) sulfate, 0.10 M

Step-by-Step Practical Procedure

  1. Place 2.0 g zinc granules in each of two test tubes.
  2. Add 10 mL of 1.0 M H2SO4 to both; add 5 drops of CuSO4 solution to one only.
  3. Start timing and observe the H2 evolution in each.
  4. Time how long each takes to produce a fixed gas volume (or compare bubble rates).
  5. Note the copper plating on the catalysed zinc.

Observations & Expected Results

Typical student data: the Cu2+-treated zinc effervesces vigorously at once and turns pink-brown with plated copper; the untreated zinc reacts sluggishly.

Worked Stoichiometric Calculations

Problem: Typical student data: 20 mL H2 collected in 300 s (uncatalysed) versus 40 s (catalysed). By what factor does Cu2+ speed the reaction?

Working: Rate ratio = 300/40 = 7.5: the copper-treated zinc reacts about 7.5 times faster.

Safety Precautions & Hazard Control

  • H2 is flammable; no flames.
  • Sulfuric acid is corrosive; wear goggles.
  • Use only drops of CuSO4; it is the catalyst.

Waste Disposal Protocol

Decant the zinc sulfate solution to the sink; collect zinc residues for the metal waste.

Viva Voce Oral Defense Questions & Answers

Q: How does Cu2+ catalyse the reaction?

A: Copper plates onto zinc forming a galvanic cell: zinc dissolves anodically while H+ is reduced on the copper cathodic sites, a lower-barrier path.

Q: Is Cu2+ consumed?

A: No: it plates out but the copper metal persists as the cathodic surface, so a trace does the job.

Q: Why is pure zinc slow?

A: A protective layer and a high hydrogen overpotential on zinc make direct H+ reduction slow.