CHEMVEN

Throwing Power of an Electroplating Bath (Haring-Blum Cell)

To measure the throwing power of a copper plating bath with the Haring-Blum cell.

Level: UniversitySafety: Needs supervisionTime: 75 min
Aim of Experiment: To measure the throwing power of a copper plating bath with the Haring-Blum cell.

Theoretical Foundations

Throwing power = (K - M)/(K + M - 2) x 100%, where K is the distance ratio of the two cathodes from the anode and M is the mass ratio of their deposits. Good throwing power (uniform deposits in recesses) comes from high cathode polarisation and conductivity.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Haring-Blum cell (long box)
  • Copper anode (centre)
  • Two copper cathodes at 1:5 distances
  • DC supply
  • Ammeter
  • Balance

Chemical Reagents

  • Acid copper sulphate bath
  • Distilled water (for rinsing)
  • Dilute H2SO4 (bath make-up acid)

Step-by-Step Practical Procedure

  1. Weigh both cathodes.
  2. Place them at distances in ratio 1:5 from the central anode.
  3. Plate at constant current for 30 minutes.
  4. Re-weigh each cathode.
  5. Compute M, then the throwing power.

Observations & Expected Results

Typical M ~ 2.5-3.5 for K = 5, giving throwing power ~20-40%.

Worked Stoichiometric Calculations

Problem: K = 5 and the deposit mass ratio M = 3.0. Calculate the throwing power.

Working: TP = (K - M)/(K + M - 2) x 100 = (5 - 3)/(5 + 3 - 2) x 100 = 2/6 x 100 = 33.3%.

Safety Precautions & Hazard Control

  • Keep the current constant.
  • Position the electrodes accurately.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Bath to electroplating waste.

Viva Voce Oral Defense Questions & Answers

Q: What does high throwing power mean in practice?

A: The bath plates recesses and distant areas almost as thickly as prominent areas - essential for complex shapes.

Q: How can throwing power be improved?

A: By raising bath conductivity, adding levelling agents, or using complexed metal ions that increase cathode polarisation.