CHEMVEN

Aluminium-Air Cell: A Metal-Air Battery

To build an aluminium-air cell and measure its practical voltage.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To build an aluminium-air cell and measure its practical voltage.

Theoretical Foundations

Anode: Al + 4OH- -> Al(OH)4- + 3e- (Edeg = -2.33 V in alkali); cathode: O2 + 2H2O + 4e- -> 4OH- (+0.40 V). Theoretical E ~ 2.7 V; practical open-circuit ~1.2-1.6 V due to parasitic corrosion and cathode overvoltage. The 'fuel' (Al) is consumed; the cell is mechanically recharged.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Aluminium foil anode
  • Carbon rod air cathode (porous)
  • Beaker
  • Digital voltmeter
  • Small bulb/LED

Chemical Reagents

  • Sodium hydroxide (1 M)
  • Distilled water (for dilutions)
  • Citric acid (for neutralising alkaline waste)

Step-by-Step Practical Procedure

  1. Immerse Al foil and the carbon air cathode (half exposed to air) in 1 M NaOH.
  2. Measure the open-circuit voltage.
  3. Connect the LED and observe.
  4. Note H2 bubbling on the Al (parasitic corrosion).
  5. Compare measured voltage with theory and account for losses.

Observations & Expected Results

Open-circuit ~1.4 V; LED lights; Al visibly corrodes with H2 evolution.

Worked Stoichiometric Calculations

Problem: Using Edeg(Al(OH)4-/Al) = -2.33 V and Edeg(O2/OH-) = +0.40 V, find the theoretical cell EMF.

Working: Edegcell = 0.40 - (-2.33) = 2.73 V.

Safety Precautions & Hazard Control

  • NaOH is caustic; wear gloves and eye protection.
  • Vent H2.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Neutralise the alkaline aluminate solution before disposal.

Viva Voce Oral Defense Questions & Answers

Q: Why is the practical voltage far below 2.73 V?

A: Parasitic Al corrosion sets a mixed potential, and O2 reduction on carbon has a large overvoltage.

Q: What is the great advantage of metal-air cells?

A: The cathode reactant (O2) comes from air, so the cell's energy density per mass of carried fuel is extremely high.

← Back to Experiments Directory