CHEMVEN

Anodising Aluminium for Corrosion Protection

To anodise aluminium, thickening its protective oxide film electrolytically.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To anodise aluminium, thickening its protective oxide film electrolytically.

Theoretical Foundations

Aluminium is the anode in dilute H2SO4: 2Al + 3H2O -> Al2O3 + 6H+ + 6e-. The porous Al2O3 layer grows outward; sealing in boiling water closes the pores. The film is hard, insulating and corrosion-resistant, and takes up dyes.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Aluminium strip (anode)
  • Lead or graphite cathode
  • Beaker
  • DC supply
  • Ammeter
  • Dye bath (optional)

Chemical Reagents

  • Sulphuric acid (1.5 M)
  • Fabric dye (optional)
  • Distilled water (for rinsing glassware and electrodes)

Step-by-Step Practical Procedure

  1. Degrease the Al strip in warm detergent and rinse.
  2. Anodise at ~1.5 A/dm2 for 30 minutes in 1.5 M H2SO4.
  3. Rinse and optionally dye in hot dye solution.
  4. Seal by boiling in distilled water for 15 minutes.
  5. Compare corrosion resistance with untreated Al in salt water.

Observations & Expected Results

Dull grey adherent oxide film; dyed samples take strong colour; anodised strip resists salt-water pitting far better.

Worked Stoichiometric Calculations

Problem: An Al strip of area 20 cm2 (one side) is anodised at 0.30 A for 30 min. What mass of Al2O3 forms? (M = 102, 6e- per Al2O3)

Working: Q = 0.30 x 1800 = 540 C. Moles e- = 540/96485 = 0.005597 mol. Moles Al2O3 = 0.005597/6 = 0.000933 mol. Mass = 0.000933 x 102 = 0.0952 g, about 95 mg.

Safety Precautions & Hazard Control

  • H2SO4 is corrosive; wear gloves and eye protection.
  • Keep the cathode from touching the anode.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Neutralise the acid bath before disposal.

Viva Voce Oral Defense Questions & Answers

Q: Why is aluminium the anode and not the cathode?

A: Oxide grows by oxidation of Al; as cathode it would just evolve H2 with no film growth.

Q: What does sealing in boiling water do?

A: It hydrates the porous alumina to boehmite, closing the pores and locking in dye and corrosion resistance.

← Back to Experiments Directory