CHEMVEN

Effect of pH on the Corrosion of Iron

To investigate how pH affects the corrosion rate of iron.

Level: UniversitySafety: Needs supervisionTime: 3 days (20 min setup)
Aim of Experiment: To investigate how pH affects the corrosion rate of iron.

Theoretical Foundations

Iron corrodes fastest in acid (H+ reduced at the cathode, plus oxide films dissolve). Near neutral pH, protective films slow attack. In strongly alkaline solution (pH > ~9), iron passivates. The Pourbaix diagram summarises these immunity/corrosion/passivity regions.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 4 identical iron nails
  • 4 beakers
  • pH paper
  • Analytical balance

Chemical Reagents

  • Dilute HCl (pH ~2)
  • Distilled water (pH ~7)
  • Dilute NaOH (pH ~12)
  • Tap water control

Step-by-Step Practical Procedure

  1. Adjust three beakers to pH ~2, ~7 and ~12; keep one as control.
  2. Weigh four identical nails and immerse one per beaker.
  3. After 3 days, clean, dry and re-weigh.
  4. Calculate mass loss vs pH and plot.
  5. Identify the passive region.

Observations & Expected Results

Mass loss highest at pH 2, moderate at pH 7, negligible at pH 12 (passive film).

Worked Stoichiometric Calculations

Problem: Mass losses: pH 2: 0.300 g; pH 7: 0.040 g; pH 12: 0.004 g. Express each as a percentage of the acid loss.

Working: pH 7: 0.040/0.300 x 100 = 13.3%. pH 12: 0.004/0.300 x 100 = 1.3% - alkaline passivation cuts corrosion ~75-fold versus acid.

Safety Precautions & Hazard Control

  • Handle HCl and NaOH with gloves and eye protection.
  • Rinse nails before weighing.
  • Wipe up any spills immediately and keep the bench dry.

Waste Disposal Protocol

Neutralise acid/alkali liquors before drain disposal.

Viva Voce Oral Defense Questions & Answers

Q: Why does iron passivate in strong alkali?

A: A protective Fe(OH)2/Fe2O3 film forms that blocks the anodic reaction - the passivity region of the Pourbaix diagram.

Q: Why is acid rain so damaging to iron structures?

A: Low pH both provides cathodic H+ reduction and dissolves protective oxide films, greatly accelerating attack.

← Back to Experiments Directory