CHEMVEN

Pitting versus Uniform Corrosion of Aluminium and Iron

To contrast uniform corrosion of iron with pitting corrosion of aluminium in chloride media.

Level: UniversitySafety: SafeTime: 3 days (15 min setup)
Aim of Experiment: To contrast uniform corrosion of iron with pitting corrosion of aluminium in chloride media.

Theoretical Foundations

Iron corrodes relatively uniformly in salt water. Aluminium's protective Al2O3 film is attacked locally by Cl-, giving deep pits (anodic sites) while the surrounding surface stays passive - small anode/large cathode geometry makes pits grow fast.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Iron nail
  • Aluminium strip
  • 2 beakers
  • Magnifying glass

Chemical Reagents

  • Sodium chloride solution (3.5%)
  • Distilled water (for rinsing glassware and electrodes)
  • Sodium bicarbonate (for neutralising small spills)

Step-by-Step Practical Procedure

  1. Immerse the nail and the Al strip in separate beakers of salt water.
  2. Observe daily with the magnifying glass.
  3. Note the distribution: uniform rust vs isolated pits with white product.
  4. Record which metal loses integrity first at local points.

Observations & Expected Results

Iron: uniform brown rust layer. Aluminium: bright overall but with small deep pits surrounded by white Al(OH)3 rings.

Worked Stoichiometric Calculations

Problem: A pit of 1 mm2 area carries 1 mA of anodic current. What is the anodic current density, and why is pitting dangerous?

Working: Current density = 1 mA/0.01 cm2 = 100 mA/cm2 - extremely high. Pitting is dangerous because deep penetration occurs with little visible mass loss or warning.

Safety Precautions & Hazard Control

  • Do not touch pits with bare fingers (oils affect observation).
  • Label beakers.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Salt solutions to drain; metals to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is pitting more dangerous than uniform corrosion?

A: It perforates the metal locally while total mass loss looks negligible, so failure comes without warning.

Q: Why does stainless steel pit in seawater?

A: Chloride breaks down its passive chromium oxide film at weak points, the same mechanism as with aluminium.