CHEMVEN

Corrosion Inhibitors: Chromate versus Oil Coating

To compare anodic inhibitor, barrier coating and unprotected iron in salt water.

Level: UniversitySafety: Needs supervisionTime: 3 days (20 min setup)
Aim of Experiment: To compare anodic inhibitor, barrier coating and unprotected iron in salt water.

Theoretical Foundations

Anodic inhibitors (e.g. chromate, nitrite) passivate the metal by forming a protective oxide film. Barrier coatings (oil/paint) physically block the electrolyte. Both reduce the corrosion current, but inhibitors work even at defects while barriers fail if breached.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 3 iron nails
  • 3 beakers
  • Sandpaper (for cleaning nails)
  • Marker pen and labels

Chemical Reagents

  • Sodium chloride (3.5%)
  • Sodium nitrite solution (0.1 M, safer inhibitor)
  • Machine oil

Step-by-Step Practical Procedure

  1. Leave nail 1 bare in salt water (control).
  2. Soak nail 2 in 0.1 M NaNO2, then place in salt water.
  3. Coat nail 3 thinly with oil, then place in salt water.
  4. Observe over 3 days and rank protection.

Observations & Expected Results

Control rusts heavily; nitrite-treated nail shows only slight staining; oiled nail stays bright unless the film is disturbed.

Worked Stoichiometric Calculations

Problem: If the control loses 0.120 g and the inhibited nail loses 0.012 g, what is the inhibitor efficiency?

Working: Efficiency = (0.120 - 0.012)/0.120 x 100 = 90%. The inhibitor cuts corrosion to one-tenth.

Safety Precautions & Hazard Control

  • Nitrite is toxic if ingested; wear gloves.
  • Handle oil with care to avoid spills.
  • Wash hands thoroughly after handling chemicals.

Waste Disposal Protocol

Nitrite solution to aqueous chemical waste, not the drain.

Viva Voce Oral Defense Questions & Answers

Q: How does nitrite inhibit corrosion?

A: It is an oxidising anodic inhibitor that helps form a passive Fe2O3 film, stifling the anodic reaction.

Q: Why is chromate being replaced by alternatives?

A: Chromate(VI) is carcinogenic; industry now uses nitrites, phosphates or organic inhibitors.