CHEMVEN

Cathodic Protection of Iron with a Magnesium Anode

To demonstrate cathodic protection using a sacrificial magnesium anode.

Level: UniversitySafety: SafeTime: 3 days (20 min setup)
Aim of Experiment: To demonstrate cathodic protection using a sacrificial magnesium anode.

Theoretical Foundations

Connecting iron to Mg (Edeg = -2.37 V) forces the iron to be the cathode of the galvanic couple (Ecell ~ 1.93 V). Oxidation occurs at the Mg anode, which is consumed instead of the iron - the principle used for pipelines and ship hulls.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Iron nail
  • Magnesium ribbon
  • Beaker
  • Connecting wire
  • Control nail in a second beaker

Chemical Reagents

  • Sodium chloride solution (3.5%)
  • Distilled water (for rinsing glassware and electrodes)
  • Sodium bicarbonate (for neutralising small spills)

Step-by-Step Practical Procedure

  1. Wire the Mg ribbon firmly to the iron nail.
  2. Immerse the couple in salt water; set up a bare control nail separately.
  3. Observe over 3 days.
  4. Record H2 bubbles on the Mg and the condition of the iron.

Observations & Expected Results

Control nail rusts; protected nail stays bright while Mg corrodes with H2 evolution.

Worked Stoichiometric Calculations

Problem: If the Mg anode loses 0.20 g (Mg -> Mg2+, M = 24.3), what charge has flowed?

Working: Moles Mg = 0.20/24.3 = 0.00823 mol. Moles e- = 0.01646 mol. Q = 0.01646 x 96485 = 1588 C, about 1.6 x 10^3 C.

Safety Precautions & Hazard Control

  • Keep Mg away from flames.
  • Ensure the wire contact stays tight.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Salt solution to drain; spent Mg to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is magnesium preferred over zinc for buried pipelines?

A: Its more negative potential drives a larger protective current through high-resistance soil.

Q: What happens when the sacrificial anode is fully consumed?

A: Protection stops and the iron begins to corrode - anodes must be inspected and replaced.

← Back to Experiments Directory