CHEMVEN

Sacrificial Protection of Iron by Zinc Coating

To demonstrate galvanised (sacrificial) protection of iron.

Level: UniversitySafety: SafeTime: 3 days (20 min setup)
Aim of Experiment: To demonstrate galvanised (sacrificial) protection of iron.

Theoretical Foundations

Zn (Edeg = -0.76 V) is more easily oxidised than Fe (Edeg = -0.44 V). When coupled, Zn becomes the anode and corrodes preferentially: Zn -> Zn2+ + 2e-, while Fe is the protected cathode. Protection continues even if the coating is scratched, unlike tin plating.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 2 iron nails
  • Zinc strip
  • 2 beakers
  • Wire

Chemical Reagents

  • Sodium chloride solution (3.5%)
  • Distilled water (for rinsing glassware and electrodes)
  • Sodium bicarbonate (for neutralising small spills)

Step-by-Step Practical Procedure

  1. Wrap one nail tightly with zinc strip, wired for good contact.
  2. Place both the wrapped nail and a bare nail in separate beakers of salt water.
  3. Observe over 3 days.
  4. Note where white Zn corrosion products versus brown rust appear.

Observations & Expected Results

Bare nail rusts heavily; zinc-wrapped nail stays bright while the zinc turns white/grey (ZnO/Zn(OH)2).

Worked Stoichiometric Calculations

Problem: Calculate Edegcell for the Zn-Fe galvanic couple and state which metal corrodes.

Working: Edegcell = Edeg(cathode) - Edeg(anode) = -0.44 - (-0.76) = +0.32 V for Zn oxidising and Fe2+ reducing. Zn is the anode and corrodes sacrificially; Fe is protected.

Safety Precautions & Hazard Control

  • Ensure good electrical contact between Zn and Fe.
  • Do not let the metals separate during the test.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Solutions to drain; metals to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why does galvanising protect even scratched steel?

A: The exposed steel is still cathodic to the surrounding zinc, so zinc corrodes instead - the protection is electrochemical, not just a barrier.

Q: Why does tin plating fail once scratched?

A: Tin (Edeg = -0.14 V) is cathodic to iron, so at a scratch the exposed iron becomes the anode and corrodes faster than bare steel.

← Back to Experiments Directory