Silver Plating a Copper Spoon

To silver-plate a copper object and determine the mass of silver deposited.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To silver-plate a copper object and determine the mass of silver deposited.

Theoretical Foundations

In a simplified argentocyanide-free bath (AgNO3 + KCN replaced by a thiosulphate complex for safety), Ag+ + e- -> Ag at the cathode. Silver's high equivalent mass (108) gives a large mass per coulomb, so thin decorative coats are easily weighed.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Copper spoon (cathode)
  • Silver anode
  • Beaker
  • DC supply (low current)
  • Balance

Chemical Reagents

  • Silver nitrate (0.1 M)
  • Sodium thiosulphate (complexing agent)
  • Sodium carbonate (cleaner)

Step-by-Step Practical Procedure

  1. Degrease the spoon in warm sodium carbonate and rinse.
  2. Weigh the spoon.
  3. Set up the bath with the spoon as cathode; plate at 0.50 A for 20 minutes.
  4. Rinse, dry and re-weigh.
  5. Compare the gain with Faraday's law and inspect the finish.

Observations & Expected Results

Bright white adherent silver coat; typical gain ~0.65-0.67 g.

Worked Stoichiometric Calculations

Problem: What mass of Ag deposits with 0.50 A for 20 minutes? (M = 108, n = 1)

Working: Q = 0.50 x 1200 = 600 C. m = 600 x 108/96485 = 64,800/96,485 = 0.671 g, about 0.67 g.

Safety Precautions & Hazard Control

  • Use low current density for a bright deposit.
  • AgNO3 stains; wear gloves.
  • Switch off the power supply before changing any connections.

Waste Disposal Protocol

Collect all silver solutions for silver recovery.

Viva Voce Oral Defense Questions & Answers

Q: Why is silver plated from a complexed bath rather than plain AgNO3?

A: Complexing lowers free [Ag+], giving slow, fine-grained, adherent deposits instead of coarse dendritic silver.

Q: Why is one electron enough per silver atom?

A: Silver deposits as Ag+ + e- -> Ag, so its equivalent mass equals its atomic mass.

← Back to Experiments Directory