Electroplating Copper onto an Iron Nail
To electroplate a uniform copper coating onto an iron nail and calculate its thickness.
Theoretical Foundations
The nail is the cathode in an acidified CuSO4 bath: Cu2+ + 2e- -> Cu. A copper anode replenishes Cu2+. The deposit mass from Faraday's law gives the mean coating thickness t = m/(rho x A) with rho(Cu) = 8.96 g/cm3.
Required Apparatus & Chemicals
Laboratory Apparatus
- Iron nail (cathode)
- Copper plate (anode)
- 250 mL beaker
- DC supply
- Ammeter
- Balance
- Sandpaper
Chemical Reagents
- CuSO4 (0.5 M) with 0.5 M H2SO4
- Distilled water (for rinsing)
- Laboratory detergent (for degreasing the nail)
Step-by-Step Practical Procedure
- Clean the nail with sandpaper, degrease, and weigh it.
- Set up the bath with the nail centred opposite the Cu anode.
- Plate at ~1.5 A for 20 minutes.
- Rinse, dry and re-weigh the nail.
- Calculate the Cu mass and estimate the coating thickness.
Observations & Expected Results
Bright adherent pink copper coating; typical mass gain ~0.59 g.
Worked Stoichiometric Calculations
Problem: A nail of surface area 12 cm2 gains 0.592 g of Cu. Estimate the coating thickness (rho = 8.96 g/cm3).
Working: Volume Cu = 0.592/8.96 = 0.0661 cm3. Thickness = V/A = 0.0661/12 = 0.00551 cm = 55 micrometres.
Safety Precautions & Hazard Control
- Degrease the nail thoroughly or the plate will peel.
- Acidic bath: wear gloves and eye protection.
- Switch off the power supply before changing any connections.
Waste Disposal Protocol
Return the plating bath to the electroplating waste bottle.
Viva Voce Oral Defense Questions & Answers
Q: Why must the nail be the cathode?
A: Reduction (Cu2+ -> Cu) occurs at the cathode; making the nail the anode would dissolve it instead.
Q: What causes a dark, powdery deposit?
A: Too high current density: H2 evolves alongside Cu, giving a spongy non-adherent plate - 'burning'.