CHEMVEN

Bakelite: Phenol-Formaldehyde Resin

To prepare Bakelite (phenol-formaldehyde thermosetting resin) under basic conditions.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To prepare Bakelite (phenol-formaldehyde thermosetting resin) under basic conditions.

Theoretical Foundations

Phenol reacts with formaldehyde (base-catalysed) to give hydroxymethyl phenols, which condense with loss of water to a cross-linked network. n C6H5OH + n HCHO -(NaOH, heat)-> cross-linked resin + n H2O. The 3D methylene-bridged network cannot be remelted - the defining property of a thermoset and the first synthetic plastic (Baekeland, 1907).

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Water bath
  • Glass stirring rod
  • Thermometer
  • Mould (e.g. bottle cap)
  • Measuring cylinders
  • Weighing balance
  • pH paper

Chemical Reagents

  • Phenol (10 g, melted)
  • Formalin, 37% formaldehyde (15 mL)
  • Sodium hydroxide (10% solution, 5 mL)
  • Concentrated HCl (for curing, few mL)
  • Distilled water

Step-by-Step Practical Procedure

  1. Melt 10 g phenol in a beaker on a water bath (fume cupboard).
  2. Add 15 mL formalin and 5 mL 10% NaOH with stirring.
  3. Heat 20-30 min; the mixture turns pink then thickens (resole stage).
  4. Pour into a mould; add a few drops of conc. HCl to accelerate curing.
  5. Cure on the water bath 30-45 min until hard.
  6. Cool, remove from the mould; note hardness and infusibility.
  7. Test: the resin does not melt on heating (chars instead).

Observations & Expected Results

Hard, glossy, pinkish-brown solid; typical yield 12-15 g. Insoluble, infusible - try heating a chip: it chars rather than melts.

Worked Stoichiometric Calculations

Problem: 10 g phenol (M = 94.11) reacts with excess formaldehyde. Assuming one CH2 bridge per phenol (net addition of CH2, M = 14.03 per unit), estimate the theoretical resin mass.

Working: Moles phenol = 10 / 94.11 = 0.1063 mol. Each phenol gains ~CH2 (14.03) minus H2O lost in condensation; approximate repeat mass = 94.11 + 30.03 - 18.02 = 106.12. Theoretical = 0.1063 x 106.12 = 11.28 g (actual crude mass is higher due to retained water/oligomers).

Safety Precautions & Hazard Control

  • Phenol is corrosive and toxic by skin absorption - gloves, fume cupboard.
  • Formaldehyde vapours are irritating and sensitising.
  • The curing exotherm can be strong in bulk - use small quantities.
  • Conc. HCl corrosive; add dropwise.

Waste Disposal Protocol

Uncured resin residues: allow to fully harden, then general solid waste. Phenol/formaldehyde liquors to toxic organic waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is Bakelite called a thermosetting plastic?

A: Its 3D cross-linked network cannot flow on heating; it chars instead of melting.

Q: What links the phenol rings?

A: Methylene (-CH2-) bridges formed by condensation of hydroxymethyl groups.

Q: How does acid vs base catalysis differ?

A: Base gives resoles (cross-link on heating); acid gives novolacs (need added hardener).

← Back to Experiments Directory