CHEMVEN

Nylon-6,6: Interfacial Polymerisation

To prepare nylon-6,6 by interfacial polymerisation of hexamethylenediamine and adipoyl chloride.

Level: UniversitySafety: Needs supervisionTime: 45 min
Aim of Experiment: To prepare nylon-6,6 by interfacial polymerisation of hexamethylenediamine and adipoyl chloride.

Theoretical Foundations

A diamine in water and a diacid chloride in an immiscible solvent react at the interface by nucleophilic acyl substitution. n H2N(CH2)6NH2 + n ClOC(CH2)4COCl -> [-NH(CH2)6NHCO(CH2)4CO-]n + 2n HCl. Polymer forms as a film that can be continuously drawn out - the classic 'nylon rope trick'.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Glass stirring rod / tweezers
  • Measuring cylinders
  • Glass rod for winding
  • Weighing balance
  • Watch glass
  • pH paper
  • Wash bottle

Chemical Reagents

  • Hexamethylenediamine (2.5 g)
  • Adipoyl chloride (2 mL)
  • Cyclohexane (50 mL)
  • Sodium hydroxide (for diamine solution)
  • Distilled water
  • Phenolphthalein (optional)

Step-by-Step Practical Procedure

  1. Dissolve 2.5 g hexamethylenediamine and 1 g NaOH in 50 mL water in a beaker.
  2. Carefully layer 2 mL adipoyl chloride in 50 mL cyclohexane on top - do not mix.
  3. A white film forms at the interface.
  4. Grasp the film with tweezers and draw it steadily upward as a continuous rope.
  5. Wind the rope on a glass rod; keep drawing until the film stops forming.
  6. Wash the nylon with water, press dry.
  7. Weigh the polymer; test its strength and melting behaviour.

Observations & Expected Results

White fibrous rope, typically 2-4 g of nylon-6,6. Strong, flexible fibres; melts around 265 C. The demonstration is visually striking.

Worked Stoichiometric Calculations

Problem: 2.5 g hexamethylenediamine (M = 116.21) reacts with excess adipoyl chloride. The repeat unit of nylon-6,6 has M = 226.32. Calculate the theoretical polymer mass and % yield for 2.8 g of rope.

Working: Moles diamine = 2.5 / 116.21 = 0.0215 mol = moles of repeat units. Theoretical polymer = 0.0215 x 226.32 = 4.87 g. % yield = (2.8 / 4.87) x 100 = 57.5% (mechanical losses during drawing are normal).

Safety Precautions & Hazard Control

  • Adipoyl chloride is corrosive and lachrymatory - fume cupboard, gloves.
  • Hexamethylenediamine is corrosive to skin and eyes.
  • Cyclohexane is highly flammable - no flames.
  • HCl is liberated; the NaOH scavenges it.

Waste Disposal Protocol

Cyclohexane layer to halogen-free organic waste. Aqueous diamine layer: neutralise before drain. Nylon rope is general solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why does polymer form only at the interface?

A: The monomers are in immiscible phases; they meet and react only at the boundary, and the film is continuously removed.

Q: What type of polymerisation is this?

A: Step-growth (condensation) polymerisation - an amide-forming nucleophilic acyl substitution.

Q: Why is NaOH added to the aqueous layer?

A: It neutralises the HCl by-product, preventing protonation of the diamine.

← Back to Experiments Directory