CHEMVEN

Gypsum (Calcium Sulfate Dihydrate) by Precipitation

To prepare gypsum by double decomposition of calcium chloride and sodium sulfate.

Level: UniversitySafety: SafeTime: 30 min
Aim of Experiment: To prepare gypsum by double decomposition of calcium chloride and sodium sulfate.

Theoretical Foundations

Calcium chloride with sodium sulfate precipitates gypsum: CaCl2 + Na2SO4 + 2H2O → CaSO4·2H2O↓ + 2NaCl. The product is chemically identical to natural gypsum used in plaster and cement.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Glass rod
  • Funnel
  • Filter paper
  • Weighing balance
  • Oven

Chemical Reagents

  • Calcium chloride dihydrate, CaCl2·2H2O (14.70 g)
  • Anhydrous sodium sulfate, Na2SO4 (14.20 g)
  • Distilled water (200 mL)

Step-by-Step Practical Procedure

  1. Dissolve 14.70 g CaCl2·2H2O in 100 mL water.
  2. Dissolve 14.20 g Na2SO4 in 80 mL water.
  3. Mix the solutions with stirring; a white precipitate forms.
  4. Allow to stand 15 minutes for complete precipitation.
  5. Filter, wash with cold water.
  6. Dry at 60 °C (not higher) and weigh.

Observations & Expected Results

White soft powder; typical yield 15.8–16.7 g.

Worked Stoichiometric Calculations

Problem: 14.70 g CaCl2·2H2O (M = 147.02) reacts with excess Na2SO4. Calculate the theoretical yield of gypsum CaSO4·2H2O (M = 172.17). If 16.2 g is obtained, find the percentage yield.

Working: Moles CaCl2·2H2O = 14.70/147.02 = 0.100 mol → 0.100 mol gypsum. Theoretical mass = 0.100 × 172.17 = 17.2 g. Percentage yield = (16.2/17.2) × 100 = 94.2%.

Safety Precautions & Hazard Control

  • Dry below 80 °C; higher temperature converts gypsum to plaster.
  • Wash free of NaCl.
  • Allow complete precipitation before filtering.
  • No special hazards.

Waste Disposal Protocol

Sodium chloride filtrate is flushed with water; non-hazardous.

Viva Voce Oral Defense Questions & Answers

Q: Why dry below 80 °C?

A: Above ~120 °C gypsum loses water to form plaster of Paris.

Q: Write the setting reaction of plaster.

A: CaSO4·½H2O + 1½H2O → CaSO4·2H2O.

Q: Name a use of gypsum in industry.

A: Retarder in Portland cement and wallboard manufacture.

← Back to Experiments Directory