CHEMVEN

Ferric Oxide (Jeweller's Rouge) by Calcining Ferrous Sulfate

To prepare red ferric oxide by thermal decomposition of ferrous sulfate.

Level: UniversitySafety: Needs supervisionTime: 90 min
Aim of Experiment: To prepare red ferric oxide by thermal decomposition of ferrous sulfate.

Theoretical Foundations

Ferrous sulfate decomposes on strong heating, the Fe(II) being oxidized by air: 2FeSO4·7H2O →(Δ) Fe2O3 + SO2↑ + SO3↑ + 14H2O. The product is the red pigment 'rouge', used for polishing glass and metals.

Required Apparatus & Chemicals

Laboratory Apparatus

  • China dish
  • Bunsen burner / furnace
  • Glass rod
  • Weighing balance
  • Fume cupboard
  • Mortar and pestle

Chemical Reagents

  • Ferrous sulfate heptahydrate, FeSO4·7H2O (27.8 g)

Step-by-Step Practical Procedure

  1. Weigh 27.8 g ferrous sulfate into a china dish in a fume cupboard.
  2. Heat gently at first to drive off water of crystallization.
  3. Increase heating strongly; the mass turns brown then red.
  4. Continue until no more fumes evolve and the mass is uniformly red.
  5. Cool, grind to a fine powder, and weigh.
  6. Test: the powder is insoluble in water but dissolves in hot concentrated HCl.

Observations & Expected Results

Fine red powder; typical yield 7.2–7.8 g; polishes glass.

Worked Stoichiometric Calculations

Problem: 27.8 g FeSO4·7H2O (M = 278.01) is calcined completely. Calculate the theoretical yield of Fe2O3 (M = 159.69). If 7.4 g is obtained, find the percentage yield.

Working: Moles FeSO4·7H2O = 27.8/278.01 = 0.100 mol. Two moles give one mole Fe2O3 = 0.050 mol. Theoretical mass = 0.050 × 159.69 = 7.98 g. Percentage yield = (7.4/7.98) × 100 = 92.7%.

Safety Precautions & Hazard Control

  • Work in a fume cupboard; SO2/SO3 fumes are toxic.
  • Heat gradually; the hydrate melts in its own water first.
  • Avoid inhaling the fine red dust.
  • Ensure complete decomposition; test for residual sulfate.

Waste Disposal Protocol

Acidic fumes are scrubbed; solid Fe2O3 is non-hazardous.

Viva Voce Oral Defense Questions & Answers

Q: Write the decomposition equation.

A: 2FeSO4 → Fe2O3 + SO2 + SO3 (from the anhydrous salt).

Q: Why is the product called jeweller's rouge?

A: The fine red powder is used for polishing jewellery and glass.

Q: What are the natural forms of Fe2O3?

A: Haematite (red) and magnetite is Fe3O4; maghemite is γ-Fe2O3.

← Back to Experiments Directory