Litharge (PbO) by Oxidation of Molten Lead
To prepare litharge by heating lead in air and skimming off the oxide layer.
Theoretical Foundations
Lead oxidizes readily in air at elevated temperature: 2Pb + O2 →(Δ) 2PbO. The yellow oxide forms a skin on molten lead; it exists as litharge (orthorhombic) when cooled slowly. Litharge is the starting material for red lead and lead glass.
Required Apparatus & Chemicals
Laboratory Apparatus
- Iron ladle or crucible
- Blast burner
- Iron skimmer
- Tongs
- Weighing balance
- Mortar and pestle
Chemical Reagents
- Lead metal pieces (20.7 g)
- Air (oxidant)
Step-by-Step Practical Procedure
- Place 20.7 g lead pieces in an iron ladle and heat strongly until molten.
- Maintain heating in air; a yellow skin of oxide forms on the surface.
- Skim off the oxide layer with an iron skimmer into a clean dish.
- Continue heating and skimming until most of the lead is oxidized.
- Cool the collected oxide, grind, and weigh.
- Store in a stoppered bottle labelled PbO.
Observations & Expected Results
Yellow powder (turns reddish on heating, yellow on cooling); typical yield 18–21 g.
Worked Stoichiometric Calculations
Problem: 20.7 g Pb (M = 207.20) is oxidized in air. Calculate the theoretical yield of litharge PbO (M = 223.20). If 19.5 g is obtained, find the percentage yield.
Working: Moles Pb = 20.7/207.20 = 0.100 mol → 0.100 mol PbO. Theoretical mass = 0.100 × 223.20 = 22.3 g. Percentage yield = (19.5/22.3) × 100 = 87.4%.
Safety Precautions & Hazard Control
- Lead and its oxide are toxic; wear gloves and a dust mask.
- Work in a ventilated area; lead fumes are hazardous.
- Handle the hot ladle with tongs only.
- Do not overheat; lead volatilizes significantly near its boiling point.
Waste Disposal Protocol
All lead residues go to the designated lead waste container.
Viva Voce Oral Defense Questions & Answers
Q: Write the formation reaction of litharge.
A: 2Pb + O2 → 2PbO.
Q: Why does litharge change colour on heating?
A: It is thermochromic: yellow at room temperature, reddish-brown when hot.
Q: Name the two crystalline forms of PbO.
A: Litharge (orthorhombic, red) and massicot (tetragonal, yellow).