Qualitative Analysis of Limestone: Calcium Carbonate

Prove a limestone chip is CaCO₃: carbonate test plus calcium confirmation, with impurity survey.

Level: UniversitySafety: Needs supervisionTime: 50 min
Aim of Experiment: Prove a limestone chip is CaCO₃: carbonate test plus calcium confirmation, with impurity survey.

Theoretical Foundations

Limestone effervesces with dilute HCl (CO₂ → milky limewater). The resulting CaCl₂ solution gives white CaC₂O₄ with ammonium oxalate and a brick-red flame. Iron impurities tint the acid extract yellow (thiocyanate test); Mg²⁺ may appear in dolomitic limestone (titan yellow after Ca removal).

Required Apparatus & Chemicals

Laboratory Apparatus

  • Test tubes
  • Mortar and pestle
  • Dropper
  • Bunsen burner + wire

Chemical Reagents

  • Limestone chips
  • Dilute HCl (~2 M)
  • Limewater
  • Ammonium oxalate
  • Aqueous NH₃
  • KSCN
  • Titan yellow
  • NaOH

Step-by-Step Practical Procedure

  1. Powder the limestone; add dilute HCl: effervescence; test gas with limewater (milky).
  2. Filter the extract; add ammonium oxalate (ammoniacal): white CaC₂O₄.
  3. Flame-test the extract: brick-red (Ca).
  4. Test the extract with KSCN: red = Fe impurity.
  5. Remove Ca as oxalate; test filtrate with titan yellow/NaOH: red = Mg (dolomitic).

Observations & Expected Results

CO₂ confirmed; Ca confirmed twice; impurity survey for Fe/Mg.

Worked Stoichiometric Calculations

Problem: 1.00 g limestone gives 0.44 g CO₂ on acid treatment. % CaCO₃? (illustrative)

Working: CaCO₃ → CO₂: 0.44 g CO₂ = 0.010 mol → 1.00 g CaCO₃ = 100% (illustrative pure sample).

Safety Precautions & Hazard Control

  • HCl corrosive — goggles.
  • Dust — avoid inhalation when powdering.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Neutralised extracts to sink; oxalate residues to chemical waste.

Viva Voce Oral Defense Questions & Answers

Q: How is limestone distinguished from dolomite here?

A: Dolomite (CaMg(CO₃)₂) gives the Mg titan-yellow test after Ca removal; pure limestone does not.

Q: Why powder the sample?

A: Surface area — coarse chips react too slowly for clean observations.

← Back to Experiments Directory