CHEMVEN

Qualitative Analysis of Brass: Copper and Zinc

Dissolve a brass sample and confirm its two major components, Cu and Zn.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: Dissolve a brass sample and confirm its two major components, Cu and Zn.

Theoretical Foundations

Brass (~60–70% Cu, ~30–40% Zn) dissolves in dilute HNO₃: Cu + 4HNO₃ → Cu(NO₃)₂ + 2NO₂ + 2H₂O; Zn similarly. Making the solution ammoniacal and adding DMG-free tests: Cu²⁺ → deep-blue [Cu(NH₃)₄]²⁺; Zn²⁺ → white K₂Zn₃[Fe(CN)₆]₂ with ferrocyanide after acidification. A real-alloy application of the schemes.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beaker
  • Test tubes
  • Fume cupboard
  • Filter paper

Chemical Reagents

  • Brass turnings/filings
  • Dilute HNO₃ (~4 M)
  • Aqueous NH₃
  • K₄[Fe(CN)₆]
  • Dilute H₂SO₄

Step-by-Step Practical Procedure

  1. Dissolve ~0.5 g brass in warm dilute HNO₃ in the fume cupboard (brown NO₂).
  2. Dilute; make ammoniacal: deep-blue solution (Cu confirmed).
  3. Acidify a portion; add ferrocyanide: white precipitate (Zn confirmed).
  4. Optional: estimate Cu:Zn roughly from colour intensity vs standards.
  5. Report the alloy composition qualitatively.

Observations & Expected Results

Blue solution (Cu); white ferrocyanide precipitate (Zn).

Worked Stoichiometric Calculations

Problem: 0.50 g brass (~65% Cu) dissolved and made to 100 mL. [Cu²⁺]? (illustrative)

Working: 0.325 g Cu = 0.0051 mol → 0.051 M — plenty for confirmatory tests.

Safety Precautions & Hazard Control

  • NO₂ evolution — fume cupboard essential.
  • HNO₃ corrosive.
  • Wear safety goggles and a lab coat throughout the experiment.

Waste Disposal Protocol

Alloy digest to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why HNO₃ and not HCl for dissolving brass?

A: HCl alone cannot oxidise copper metal; HNO₃'s oxidising power is needed.

Q: How would you detect leaded brass?

A: Dilute H₂SO₄ gives white PbSO₄ — lead is a common brass additive.