CHEMVEN

Thermite Reaction: Aluminium Reduces Iron(III) Oxide

To demonstrate the highly exothermic thermite reaction 2Al + Fe2O3 → Al2O3 + 2Fe and calculate its enthalpy.

Level: UniversitySafety: Advanced lab onlyTime: 45 min
Aim of Experiment: To demonstrate the highly exothermic thermite reaction 2Al + Fe2O3 → Al2O3 + 2Fe and calculate its enthalpy.

Theoretical Foundations

Aluminium's huge affinity for oxygen drives the reaction: 2Al + Fe2O3 → 2Fe + Al2O3, ΔH ≈ −852 kJ per mole of Fe2O3. Temperatures exceed 2000 °C, melting the iron produced — the basis of thermite welding for railway tracks. Once ignited (magnesium ribbon fuse), it cannot be stopped and needs no external oxygen.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Firebrick or sand tray
  • Crucible or flowerpot with sand base
  • Magnesium ribbon fuse
  • Long tongs
  • Face shield, heat gloves
  • Fire extinguisher (sand bucket)

Chemical Reagents

  • Aluminium powder (about 25 g)
  • Iron(III) oxide powder Fe2O3 (about 75 g)
  • Magnesium ribbon (fuse)

Step-by-Step Practical Procedure

  1. Mix 25 g Al powder with 75 g Fe2O3 thoroughly (1:3 mass ratio).
  2. Place the mix in a depression on the sand bed, away from flammables.
  3. Insert a magnesium ribbon fuse into the mix.
  4. All observers retreat behind the safety screen with face shields.
  5. Ignite the fuse with a long taper.
  6. Observe the brilliant white-hot reaction and the molten iron bead formed.

Observations & Expected Results

An intensely bright, showering reaction lasting seconds; a glowing bead of molten iron sinks into the sand, surrounded by white-hot alumina slag.

Worked Stoichiometric Calculations

Problem: For 100 g of thermite mix (25.3 g Al + 74.7 g Fe2O3), calculate the heat released (ΔH = −852 kJ per 159.69 g Fe2O3).

Working: Moles Fe2O3 = 74.7/159.69 = 0.4678 mol. Heat = 0.4678 × 852 = 399 kJ — from just 100 g of powder.

Safety Precautions & Hazard Control

  • Advanced lab only; instructor performs the ignition.
  • Full face shields and a safety screen are mandatory.
  • Never use water on the reaction; have dry sand ready.
  • Ensure no flammables within several meters; ventilate the smoke.

Waste Disposal Protocol

The cooled iron bead and slag are general waste once fully cold; sweep up unreacted powder as metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the reaction so exothermic?

A: Al2O3 has an extremely negative heat of formation (−1676 kJ mol⁻¹); aluminium 'steals' oxygen from Fe2O3.

Q: Why can't it be stopped once started?

A: It needs no air — the oxidizer (Fe2O3) is in the mix — and its own heat sustains it.

Q: Name one industrial use.

A: Welding railway rails in situ.

← Back to Experiments Directory