Goethite to Hematite: Heat Turns Yellow Ochre Red

To convert yellow iron-oxide pigment (goethite) to red hematite by heating and explain the dehydration.

Level: UniversitySafety: Needs supervisionTime: 50 min
Aim of Experiment: To convert yellow iron-oxide pigment (goethite) to red hematite by heating and explain the dehydration.

Theoretical Foundations

Yellow ochre is goethite, FeO(OH). Heating to about 250-300 °C dehydrates it: 2FeO(OH) → Fe2O3 + H2O, giving red hematite — the basis of 'burnt ochre' and 'red oxide' pigments used since prehistory. The color change reflects the different ligand-field environments of Fe³⁺ in the two structures.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Crucible
  • Bunsen burner or furnace
  • Tongs
  • White tile
  • Balance

Chemical Reagents

  • Yellow ochre / goethite pigment (about 5 g)
  • Distilled water (for making a streak paste)
  • White paper (for streak comparison)

Step-by-Step Practical Procedure

  1. Weigh 5.0 g of yellow ochre into the crucible.
  2. Heat strongly for 15 minutes with occasional stirring.
  3. Observe the color change from yellow-brown to red.
  4. Cool and reweigh to find the mass loss.
  5. Compare the loss with the theoretical dehydration loss.
  6. Smear both pigments on a white tile to compare streak colors.

Observations & Expected Results

The powder turns distinctly red ('burnt ochre'); mass drops by about 10%, matching loss of structural water.

Worked Stoichiometric Calculations

Problem: 2FeO(OH) (M = 88.85) → Fe2O3 + H2O. What is the theoretical mass loss for 5.00 g?

Working: Moles = 5.00/88.85 = 0.05627 mol. Water lost = 0.05627/2 = 0.02814 mol = 0.507 g (10.1%).

Safety Precautions & Hazard Control

  • Hot crucible: tongs and heat gloves only.
  • Pigment dust: avoid inhaling.
  • Let the crucible cool fully before handling.

Waste Disposal Protocol

Iron oxide pigments are low hazard; solids go in general waste.

Viva Voce Oral Defense Questions & Answers

Q: Write the conversion reaction.

A: 2FeO(OH) → Fe2O3 + H2O (heat).

Q: Why does the color change?

A: Fe³⁺ sits in different crystal-field environments in goethite versus hematite, shifting d-d absorption.

Q: What is 'burnt ochre'?

A: Natural yellow ochre calcined to red hematite pigment.