Lime Mortar Carbonation: How Old Buildings Harden

To follow the slow carbonation of lime mortar (Ca(OH)2 + CO2 → CaCO3) by phenolphthalein testing and hardness.

Level: UniversitySafety: SafeTime: 30 min setup + 14 days
Aim of Experiment: To follow the slow carbonation of lime mortar (Ca(OH)2 + CO2 → CaCO3) by phenolphthalein testing and hardness.

Theoretical Foundations

Lime mortar hardens not by hydration but by carbonation: calcium hydroxide reacts with atmospheric CO2 to form calcium carbonate, the same binder as in limestone. The reaction front moves inward slowly (millimeters per month); phenolphthalein stays pink where uncarbonated Ca(OH)2 remains (pH > 9) and goes colorless in carbonated zones.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Small molds or cups
  • Trowel/stick
  • Phenolphthalein spray
  • Knife

Chemical Reagents

  • Hydrated lime Ca(OH)2 (about 200 g)
  • Sharp sand (about 600 g)
  • Water
  • Phenolphthalein indicator

Step-by-Step Practical Procedure

  1. Mix 1 part lime with 3 parts sand and enough water for a workable mortar.
  2. Cast small discs and expose to air.
  3. After 3, 7, and 14 days, cut a disc and spray the fresh face with phenolphthalein.
  4. Measure the pink (uncarbonated) core versus the colorless rim.
  5. Test surface hardness by scratching over time.
  6. Plot carbonation depth versus the square root of time.

Observations & Expected Results

A colorless carbonated rim grows inward from the surface while the core stays pink; hardness increases slowly over weeks.

Worked Stoichiometric Calculations

Problem: Ca(OH)2 (M = 74.09) + CO2 → CaCO3 + H2O. What mass of CO2 is absorbed per 100 g of lime fully carbonated?

Working: Moles = 100/74.09 = 1.350 mol. CO2 = 1.350 × 44.01 = 59.4 g.

Safety Precautions & Hazard Control

  • Hydrated lime is caustic; wear gloves and goggles.
  • Avoid inhaling lime dust.
  • Wash skin after handling.

Waste Disposal Protocol

Hardened mortar is general/construction waste; wash tools before mortar sets.

Viva Voce Oral Defense Questions & Answers

Q: Write the carbonation reaction.

A: Ca(OH)2 + CO2 → CaCO3 + H2O.

Q: How does lime mortar differ from cement mortar in hardening?

A: Lime hardens by slow CO2 carbonation; cement hardens by fast hydration.

Q: Why does phenolphthalein map the reaction front?

A: Uncarbonated Ca(OH)2 keeps pH > 9 (pink); carbonated CaCO3 zones are near-neutral (colorless).