Thermal Shock: Borosilicate versus Soda-Lime Glass
To compare the thermal-shock resistance of borosilicate and soda-lime glass by quenching heated samples, relating it to thermal expansion.
Theoretical Foundations
Thermal stress σ ∝ E·α·ΔT/(1−ν). Borosilicate glass has α ≈ 3.3 × 10⁻⁶ K⁻¹ versus ≈ 9 × 10⁻⁶ K⁻¹ for soda-lime, so for the same quench it develops about one-third the stress — the reason lab glassware survives hot-to-cold shocks that shatter ordinary glass.
Required Apparatus & Chemicals
Laboratory Apparatus
- Borosilicate test tube
- Soda-lime test tube (ordinary)
- Bunsen burner
- Tongs
- Bucket of ice water
- Safety screen
Chemical Reagents
- Borosilicate test tube
- Soda-lime test tube
- Ice (for the ice-water quench bath)
Step-by-Step Practical Procedure
- Heat the soda-lime tube in the flame until hot (not softening).
- Plunge it into ice water with tongs behind the safety screen.
- Record whether it cracks.
- Repeat with the borosilicate tube under identical heating.
- Compare outcomes and relate to the α values.
- Discuss why lab glassware is borosilicate.
Observations & Expected Results
The soda-lime tube typically cracks with an audible ping; the borosilicate tube survives repeated quenches unchanged.
Worked Stoichiometric Calculations
Problem: Stress scales with α·ΔT. For ΔT = 200 K, compare the thermal strain α·ΔT for the two glasses.
Working: Borosilicate: 3.3 × 10⁻⁶ × 200 = 6.6 × 10⁻⁴. Soda-lime: 9 × 10⁻⁶ × 200 = 1.8 × 10⁻³ — about 2.7× larger strain, hence cracking.
Safety Precautions & Hazard Control
- Wear goggles and use the safety screen; glass can shatter.
- Handle hot glass only with tongs.
- Let quenched glass cool before touching.
- Bin broken glass in a sharps container.
Waste Disposal Protocol
Broken glass goes in the glass/sharps bin, not general waste.
Viva Voce Oral Defense Questions & Answers
Q: Why does borosilicate resist thermal shock?
A: Its low thermal expansion coefficient (≈ 3.3 × 10⁻⁶ K⁻¹) generates much smaller quench stresses.
Q: What does the boron do in the glass network?
A: BO3/BO4 units strengthen the silica network and lower thermal expansion.
Q: Give two lab uses of borosilicate glass.
A: Beakers/flasks that are heated, and condensers subjected to temperature gradients.