Plaster of Paris Setting: An Exothermic Hydration
To follow the setting of plaster of Paris (CaSO4·½H2O → CaSO4·2H2O) by temperature and hardness, and explain the interlocking-crystal mechanism.
Theoretical Foundations
Plaster of Paris is calcium sulfate hemihydrate. Mixed with water it dissolves and reprecipitates as gypsum dihydrate needles (CaSO4·½H2O + 1.5H2O → CaSO4·2H2O); the interlocking needles give strength, and the reaction is exothermic. Too much water gives weak, porous casts — the same w/c principle as cement.
Required Apparatus & Chemicals
Laboratory Apparatus
- Paper cups
- Balance
- Thermometer
- Stirring stick
- Stopwatch
Chemical Reagents
- Plaster of Paris (about 200 g)
- Water (about 120 mL)
- Petroleum jelly (thin mold coating, optional)
Step-by-Step Practical Procedure
- Weigh 100 g plaster into each of two cups.
- Add 60 mL water to one and 100 mL to the other; stir 1 minute.
- Record temperature every 2 minutes for 20 minutes.
- Note the time each becomes too stiff to stir (initial set).
- After 30 minutes, compare hardness by thumbnail scratch.
- Relate strength and set time to the water ratio.
Observations & Expected Results
Temperature climbs several degrees peaking near the set; the low-water cast sets faster and becomes much harder than the soupy high-water cast.
Worked Stoichiometric Calculations
Problem: What mass of water is chemically required to convert 100 g of hemihydrate (M = 145.15) fully to dihydrate?
Working: Moles = 100/145.15 = 0.689 mol. Water needed = 1.5 × 0.689 = 1.033 mol = 18.6 g — far less than mixing water; the rest is workability water that leaves pores.
Safety Precautions & Hazard Control
- Plaster dust irritates lungs; avoid inhaling.
- Wash hands after handling.
- Do not pour plaster slurry down the drain — it sets in pipes.
Waste Disposal Protocol
Let cups harden fully, then bin as general/construction waste.
Viva Voce Oral Defense Questions & Answers
Q: Write the setting reaction.
A: CaSO4·½H2O + 1.5H2O → CaSO4·2H2O.
Q: Why does the cast harden?
A: Interlocking needle crystals of gypsum grow and mat together.
Q: Why does extra water weaken plaster?
A: It leaves pores after evaporation, same as in cement.