Gold Nanoparticles: Red Sol by the Turkevich Method
To prepare a ruby-red gold nanoparticle sol by citrate reduction of chloroauric acid and relate its color to particle size.
Theoretical Foundations
The Turkevich method reduces HAuCl4 with boiling sodium citrate to give about 15-20 nm gold spheres. Their surface plasmon resonance absorbs green light near 520 nm, so the sol transmits ruby red — the same physics behind medieval ruby glass. More citrate gives smaller particles and a bluer-red color, showing size-tunable optics.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL conical flask
- Hot plate with stirrer
- Dropper
- UV-vis spectrometer (optional)
- Dark storage bottle
Chemical Reagents
- Chloroauric acid HAuCl4·3H2O (about 0.05 g) or 1 mM solution
- Sodium citrate 1% solution (about 5 mL)
- Distilled water (about 100 mL)
Step-by-Step Practical Procedure
- Bring 100 mL of 1 mM HAuCl4 to a rolling boil with stirring.
- Inject 5 mL of 1% sodium citrate rapidly.
- Watch the color sequence: yellow → colorless → blue-grey → wine red over 2-3 minutes.
- Boil 10 minutes more, then cool.
- Record the plasmon peak near 520 nm if possible.
- Store in the dark; note stability over days.
Observations & Expected Results
The solution passes through transient blue-grey (aggregating nuclei) and settles to a clear ruby-red sol with a plasmon band near 520 nm.
Worked Stoichiometric Calculations
Problem: A 15 nm gold sphere contains roughly 100,000 Au atoms. If the sol is 1 mM in Au atoms, what is the particle (not atom) concentration?
Working: 1 mM atoms / 10⁵ atoms per particle = 10⁻⁸ M = 10 nM in particles.
Safety Precautions & Hazard Control
- HAuCl4 is corrosive and stains; wear gloves and goggles.
- Boiling acid solutions: use a stirrer to prevent bumping.
- Do not ingest the sol.
- Work in a ventilated area.
Waste Disposal Protocol
Collect gold-containing waste for precious-metal recovery; never pour down the drain.
Viva Voce Oral Defense Questions & Answers
Q: Why is the sol red?
A: 15-20 nm gold spheres absorb green (~520 nm) by surface plasmon resonance, transmitting red.
Q: What causes the transient blue-grey stage?
A: Nuclei briefly aggregate into larger clusters (absorbing redder light) before citrate capping stabilizes small spheres.
Q: How does citrate amount affect size?
A: More citrate → more nuclei → smaller final particles.