Silver Nanoparticles: Yellow Sol by Citrate Reduction
To synthesize a yellow colloidal sol of silver nanoparticles by citrate reduction and explain its color by surface plasmon resonance.
Theoretical Foundations
Boiling AgNO3 with sodium citrate reduces Ag⁺ to Ag⁰; citrate also caps the particles, arresting growth at about 20-60 nm. Particles much smaller than light's wavelength show surface plasmon resonance — collective electron oscillation — absorbing near 400-420 nm, so the transmitted sol looks yellow. This is the basis of the classic photographic and antimicrobial silver colloids.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL conical flask
- Hot plate with magnetic stirrer
- Burette or dropper
- UV-vis spectrometer or colorimeter (optional)
- Cuvettes
Chemical Reagents
- Silver nitrate AgNO3 (about 0.09 g for 500 mL of 1 mM)
- Sodium citrate dihydrate (1% solution, about 10 mL)
- Distilled water (about 200 mL)
Step-by-Step Practical Procedure
- Dissolve 0.034 g AgNO3 in 200 mL distilled water (1 mM) and bring to a rolling boil with stirring.
- Add 4 mL of 1% sodium citrate solution dropwise.
- Keep boiling 10 minutes; the solution turns pale yellow, deepening with time.
- Cool and store the sol in a dark bottle.
- Record the absorption maximum (about 400-420 nm) if a spectrometer is available.
- Compare the color with bulk silver to discuss the nanoscale optical effect.
Observations & Expected Results
The colorless solution turns clear yellow with no precipitate; the spectrum shows a sharp plasmon band near 410 nm, characteristic of spherical Ag nanoparticles.
Worked Stoichiometric Calculations
Problem: What mass of AgNO3 (M = 169.87) is needed for 200 mL of 1.0 mM solution?
Working: Moles = 0.200 × 0.001 = 2.0 × 10⁻⁴ mol. Mass = 2.0 × 10⁻⁴ × 169.87 = 0.034 g.
Safety Precautions & Hazard Control
- Silver nitrate stains skin and is toxic; wear gloves.
- Boiling solutions can bump; use a stirrer.
- Do not ingest the nanoparticle sol.
- Keep the sol away from drains in quantity — collect if required locally.
Waste Disposal Protocol
Collect the silver sol as heavy-metal/nanomaterial waste per local rules; do not pour concentrated sol down the drain.
Viva Voce Oral Defense Questions & Answers
Q: Why is the sol yellow although bulk silver is metallic grey?
A: Nanoscale silver absorbs blue light (~410 nm) by surface plasmon resonance; the transmitted color is yellow.
Q: What two roles does citrate play?
A: Reducing agent (Ag⁺ → Ag⁰) and capping agent that stops particle growth.
Q: Why must the particles stay below ~100 nm?
A: Plasmon resonance and stable colloidal behavior occur only when particles are much smaller than the wavelength of light.