NTC Thermistor: Semiconductor Resistance Falls with Temperature

To measure the resistance-temperature curve of an NTC thermistor and determine its material constant B.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To measure the resistance-temperature curve of an NTC thermistor and determine its material constant B.

Theoretical Foundations

In a semiconductor, heating excites more electrons across the band gap, so conductivity rises and resistance falls — opposite to metals. An NTC thermistor follows R = R0·exp[B(1/T − 1/T0)]. Plotting ln R against 1/T gives a straight line of slope B (typically 3000-5000 K), the basis of thermistor thermometry.

Required Apparatus & Chemicals

Laboratory Apparatus

  • NTC thermistor (10 kΩ at 25 °C)
  • Digital multimeter
  • Water bath with heater
  • Thermometer (0-100 °C)
  • Beaker
  • Sealed plastic bag for thermistor

Chemical Reagents

  • Water for the bath
  • Ice (for low-temperature points)
  • Table salt (optional, to depress the ice-bath temperature)

Step-by-Step Practical Procedure

  1. Seal the thermistor in a thin plastic bag with its leads out.
  2. Immerse it in a water bath with the thermometer bulb beside it.
  3. Record resistance at 10 °C intervals from about 10 °C to 80 °C.
  4. Plot ln R versus 1/T (T in kelvin).
  5. Find the slope B from the best-fit line.
  6. Use B to predict R at 50 °C and check against measurement.

Observations & Expected Results

Resistance drops from tens of kΩ near 0 °C to a few kΩ near 80 °C; the ln R vs 1/T plot is linear, giving B ≈ 3950 K.

Worked Stoichiometric Calculations

Problem: An NTC thermistor has R0 = 10 kΩ at 25 °C (298 K) and B = 3950 K. Calculate R at 50 °C (323 K).

Working: R = 10 × exp[3950 × (1/323 − 1/298)] = 10 × exp[3950 × (−2.598 × 10⁻⁴)] = 10 × exp(−1.026) = 10 × 0.358 = 3.58 kΩ.

Safety Precautions & Hazard Control

  • Keep the multimeter and leads dry; seal the thermistor well.
  • Handle hot water carefully.
  • Do not exceed the thermistor's rated temperature.

Waste Disposal Protocol

No chemical waste; water goes down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why does a semiconductor's resistance fall with temperature?

A: More electrons are thermally excited across the band gap, increasing charge carriers.

Q: How does this differ from a metal?

A: In metals, heating increases lattice vibrations that scatter electrons, so resistance rises.

Q: What is the B constant?

A: The material constant in R = R0·exp[B(1/T − 1/T0)]; larger B means steeper temperature sensitivity.