Passivation of Aluminium: The Invisible Oxide Shield
To demonstrate that aluminium's corrosion resistance comes from a thin adherent Al2O3 film, by comparing etched and filmed aluminium in salt water and with mercury.
Theoretical Foundations
Aluminium is very reactive (E° = −1.66 V) but resists corrosion because a 2-5 nm film of Al2O3 forms instantly in air and seals the surface. Removing the film with NaOH exposes active metal that reacts vigorously; mercury amalgamates aluminium and prevents film repair, causing rapid 'mercury corrosion' — which is why mercury is banned from aircraft.
Required Apparatus & Chemicals
Laboratory Apparatus
- 2 beakers
- Aluminium foil strips
- Tweezers
- Dropper
Chemical Reagents
- Sodium hydroxide solution, about 1 M (a few mL)
- Salt water (a few mL)
- Dilute hydrochloric acid (a few drops, optional)
Step-by-Step Practical Procedure
- Place two aluminium strips in salt water; note the lack of reaction (passive film intact).
- Dip one strip briefly in 1 M NaOH to strip the oxide, rinse, and return it to salt water.
- Observe the difference in bubbling/corrosion between etched and unetched strips.
- On a third strip, scratch through the film under a drop of dilute HCl and watch.
- Note how quickly the film reforms in air (repassivation).
Observations & Expected Results
Untouched aluminium is inert; the NaOH-etched strip fizzes and dulls as fresh metal corrodes before the film reforms; the scratched spot under acid bubbles briefly then repassivates.
Worked Stoichiometric Calculations
Problem: The passive film is about 4 nm thick on 1 cm² of aluminium. What is the film volume, and what mass of Al2O3 does it contain? (ρ ≈ 3.97 g cm⁻³)
Working: Volume = 1 cm² × 4 × 10⁻⁷ cm = 4 × 10⁻⁷ cm³. Mass = 4 × 10⁻⁷ × 3.97 = 1.6 × 10⁻⁶ g — about 1.6 µg, showing how little oxide gives full protection.
Safety Precautions & Hazard Control
- NaOH is caustic; wear goggles and gloves.
- Do NOT use mercury in this demonstration — discuss the mercury effect theoretically only.
- Rinse skin immediately if splashed.
Waste Disposal Protocol
Neutralize the NaOH washings before drain disposal; aluminium strips go in metal recycling.
Viva Voce Oral Defense Questions & Answers
Q: What is passivation?
A: Formation of a thin, adherent, protective oxide film that blocks further corrosion.
Q: Why is aluminium corrosion-resistant despite E° = −1.66 V?
A: Kinetics, not thermodynamics: the instant Al2O3 film isolates the metal from the environment.
Q: Why is mercury forbidden near aluminium aircraft?
A: It amalgamates aluminium, preventing the protective film from reforming, causing rapid crumbling corrosion.