CHEMVEN

Corrosion Inhibitors: Slowing Rust with Sodium Benzoate

To compare the effectiveness of anodic inhibitor (sodium nitrite) and adsorption inhibitor (sodium benzoate) against a control.

Level: UniversitySafety: Needs supervisionTime: 20 min setup + 7 days observation
Aim of Experiment: To compare the effectiveness of anodic inhibitor (sodium nitrite) and adsorption inhibitor (sodium benzoate) against a control.

Theoretical Foundations

Corrosion inhibitors adsorb on the metal or stabilize passive films. Sodium nitrite is an anodic passivator that helps form a protective γ-Fe2O3 film; sodium benzoate adsorbs on the surface blocking active sites. Inhibitor efficiency is judged by the reduction in rusted area versus an untreated control in the same electrolyte.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 3 beakers
  • 3 iron nails
  • Balance
  • Salt water

Chemical Reagents

  • Sodium chloride solution, 3.5% (about 600 mL)
  • Sodium nitrite (about 2 g)
  • Sodium benzoate (about 2 g)
  • Iron nails (3)

Step-by-Step Practical Procedure

  1. Prepare 200 mL of 3.5% NaCl in each of three beakers.
  2. To beaker 2 add 1% sodium nitrite; to beaker 3 add 1% sodium benzoate; beaker 1 is the control.
  3. Immerse one weighed nail in each.
  4. Leave for 7 days at room temperature.
  5. Remove, dry, and compare rust coverage; reweigh to estimate mass loss.
  6. Calculate inhibitor efficiency = (loss(control) − loss(inhibited))/loss(control) × 100%.

Observations & Expected Results

The control rusts heavily; both inhibited nails show far less rust, with the nitrite sample often nearly bright due to passivation.

Worked Stoichiometric Calculations

Problem: Mass losses: control 0.42 g, nitrite 0.05 g, benzoate 0.12 g. Calculate each inhibitor's efficiency.

Working: Nitrite: (0.42 − 0.05)/0.42 × 100% = 88%. Benzoate: (0.42 − 0.12)/0.42 × 100% = 71%.

Safety Precautions & Hazard Control

  • Sodium nitrite is toxic if ingested; wear gloves.
  • Do not acidify nitrite solutions (nitrous fumes).
  • Wash hands after handling.

Waste Disposal Protocol

Dilute solutions may go down the drain with plenty of water; nails to recycling.

Viva Voce Oral Defense Questions & Answers

Q: What is an anodic inhibitor?

A: A chemical that suppresses the anodic dissolution reaction, often by stabilizing a passive oxide film.

Q: Why is too little inhibitor dangerous?

A: Partial coverage can create small anodes and large cathodes, causing intense localized (pitting) attack.

Q: Name an industrial use of inhibitors.

A: Cooling-water systems, oil pipelines, concrete rebar protection, antifreeze formulations.

← Back to Experiments Directory