Galvanic Corrosion: The Iron-Copper Couple
To show that connecting iron to copper in salt water accelerates iron corrosion, and to measure the galvanic current.
Theoretical Foundations
Iron (E° = −0.44 V) coupled to copper (E° = +0.34 V) forms a galvanic cell with EMF ≈ 0.78 V. Iron becomes the anode and dissolves faster than it would alone, while hydrogen/oxygen reduction occurs on the copper cathode. This is why dissimilar-metal contacts in structures must be insulated.
Required Apparatus & Chemicals
Laboratory Apparatus
- Beaker
- Iron nail
- Copper strip
- Connecting wire
- Milliammeter (0-10 mA)
- Salt water (3.5% NaCl)
- Sandpaper
Chemical Reagents
- Sodium chloride solution, 3.5% (about 250 mL)
- Iron nail
- Copper strip
Step-by-Step Practical Procedure
- Clean both metals with sandpaper.
- Immerse the nail and copper strip separately in salt water, not touching.
- Connect them through the milliammeter and record the current.
- Note which electrode is positive (copper) and which corrodes (iron).
- Leave coupled for 30 min and observe rust forming on the iron near the junction.
- Compare with an uncoupled control nail.
Observations & Expected Results
A current of typically 0.5-3 mA flows from copper to iron through the meter; rust blooms rapidly on the iron, especially near the copper contact, while the copper stays bright.
Worked Stoichiometric Calculations
Problem: If the cell EMF is 0.78 V and the measured current is 2.0 mA, what is the total cell resistance?
Working: R = V/I = 0.78/(2.0 × 10⁻³) = 390 Ω — mostly the electrolyte and polarization resistance.
Safety Precautions & Hazard Control
- Keep the meter dry.
- Salt water is low hazard.
- Sand metal away from the face to avoid dust in eyes.
Waste Disposal Protocol
Salt water down the drain; metals go to recycling.
Viva Voce Oral Defense Questions & Answers
Q: Which metal corrodes in the Fe-Cu couple and why?
A: Iron — it is the more anodic metal (more negative E°), so it oxidizes.
Q: What is the theoretical EMF of the Fe-Cu cell?
A: E°(Cu) − E°(Fe) = 0.34 − (−0.44) = 0.78 V.
Q: How is galvanic corrosion prevented in practice?
A: Insulate dissimilar metals, use compatible metals, or apply cathodic protection.