Identifying an Alloy by Density: Is It Really Brass?
To determine the density of an unknown copper-alloy sample by Archimedes' principle and identify it as brass, bronze, or copper.
Theoretical Foundations
Archimedes' principle: the apparent loss of weight in water equals the weight of displaced water, so density = W(air)/(W(air) − W(water)) × ρ(water). Copper (8.96), bronze (about 8.8), and brass (about 8.4 g cm⁻³) are close but distinguishable with careful weighing, showing how density fingerprints alloys.
Required Apparatus & Chemicals
Laboratory Apparatus
- Balance (0.01 g)
- Beaker of distilled water
- Thin thread
- Unknown alloy samples (labeled A, B, C)
- Calipers (optional)
Chemical Reagents
- Distilled water
- Unknown copper-alloy samples
- Detergent (a drop, anti-bubble)
Step-by-Step Practical Procedure
- Weigh the dry sample in air: W(air).
- Suspend it by thread in water (fully immersed, not touching the beaker) and weigh: W(water).
- Compute ρ = W(air)/(W(air) − W(water)) × 0.998 g cm⁻³.
- Repeat for each unknown.
- Compare with reference densities: Cu 8.96, bronze about 8.8, brass about 8.4.
- Assign each unknown and estimate confidence from the spread of repeats.
Observations & Expected Results
The three unknowns separate into groups near 8.9, 8.8, and 8.4 g cm⁻³, allowing identification as copper, bronze, and brass.
Worked Stoichiometric Calculations
Problem: A sample weighs 45.20 g in air and 39.82 g in water. Calculate its density and identify it.
Working: ρ = 45.20/(45.20 − 39.82) × 0.998 = 45.20/5.38 × 0.998 = 8.38 g cm⁻³ — consistent with brass.
Safety Precautions & Hazard Control
- Remove air bubbles clinging to the sample before weighing in water.
- Keep water at room temperature.
- Dry samples after the test to prevent tarnishing.
Waste Disposal Protocol
No waste; water goes down the drain and samples are reused.
Viva Voce Oral Defense Questions & Answers
Q: State Archimedes' principle.
A: A body immersed in fluid experiences an upthrust equal to the weight of displaced fluid.
Q: Why must the sample not touch the beaker?
A: Contact adds a reaction force that falsifies the apparent weight in water.
Q: Why is temperature noted?
A: Water density changes slightly with temperature, affecting the result.