CHEMVEN

Solder Alloys: How Composition Controls the Melting Range

To compare the melting behavior of 60/40 Sn-Pb solder with pure tin and pure lead and locate the near-eutectic composition.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To compare the melting behavior of 60/40 Sn-Pb solder with pure tin and pure lead and locate the near-eutectic composition.

Theoretical Foundations

The tin-lead phase diagram has a eutectic at 61.9% Sn and 183 °C — the lowest melting point in the system. Near-eutectic 60/40 solder melts sharply at about 183-190 °C, far below tin (232 °C) or lead (327 °C). Off-eutectic alloys melt over a pasty range between solidus and liquidus, which is why plumbers once preferred them and electronics prefers eutectic solder.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Soldering iron or small furnace
  • Crucible
  • Thermocouple or thermometer (to 350 °C)
  • Samples: Sn wire, Pb sheet, 60/40 solder wire
  • Tongs
  • Heat-resistant mat

Chemical Reagents

  • Tin sample (a few grams)
  • Lead sample (a few grams, handle with gloves)
  • 60/40 Sn-Pb solder (a few grams)

Step-by-Step Practical Procedure

  1. Record the handbook melting points: Sn 232 °C, Pb 327 °C, eutectic 183 °C.
  2. Heat each sample separately in the crucible with the thermocouple attached.
  3. Note the temperature at which each sample first softens and fully liquefies.
  4. Observe the pasty range of any off-eutectic behavior.
  5. Compare the sharp melting of 60/40 solder with the pure metals.
  6. Sketch the observed melting ranges on a temperature-composition diagram.

Observations & Expected Results

Pure tin and lead melt sharply at 232 °C and 327 °C; the 60/40 solder collapses to liquid at about 183-190 °C with almost no pasty range.

Worked Stoichiometric Calculations

Problem: The Sn-Pb eutectic is 61.9% Sn at 183 °C. How much lower is this than the melting point of pure lead (327 °C)?

Working: 327 − 183 = 144 °C lower — alloying depresses the melting point dramatically at the eutectic.

Safety Precautions & Hazard Control

  • Lead is toxic; wear gloves and do not ingest or inhale fumes.
  • Work in a ventilated area.
  • Handle hot crucibles with tongs only.
  • Wash hands thoroughly after handling lead.

Waste Disposal Protocol

Collect all lead-containing scrap as hazardous metal waste; never put lead in general waste.

Viva Voce Oral Defense Questions & Answers

Q: What is a eutectic?

A: The composition with the lowest melting point in a binary system, where liquid freezes to two solids simultaneously.

Q: Why is near-eutectic solder preferred for electronics?

A: It solidifies sharply with no pasty range, giving reliable joints.

Q: What is the pasty range?

A: The temperature interval between solidus and liquidus where solid and liquid coexist.

← Back to Experiments Directory