Making Brass: A Copper-Zinc Substitutional Alloy
To prepare a brass alloy (about 70% Cu, 30% Zn) by melting and to compare its color, hardness, and density with pure copper.
Theoretical Foundations
Brass is a substitutional solid solution: zinc atoms (radius 134 pm) replace copper atoms (128 pm) in the fcc copper lattice, distorting it and impeding dislocation motion, which hardens the alloy. Typical cartridge brass (70/30) is golden, harder than copper, and has a density of about 8.4-8.5 g cm⁻³, between copper (8.96) and zinc (7.14).
Required Apparatus & Chemicals
Laboratory Apparatus
- Furnace or crucible with burner (capable of about 1000 °C)
- Graphite or clay crucible
- Crucible tongs
- Mold (steel ingot mold)
- Balance
- File and emery paper
- Face shield, heat-resistant gloves
Chemical Reagents
- Copper pieces (about 70 g)
- Zinc pieces (about 30 g)
- Borax flux (a few grams)
Step-by-Step Practical Procedure
- Weigh 70 g of copper and 30 g of zinc.
- Melt the copper in the crucible with a pinch of borax flux to prevent oxidation.
- Add the zinc pieces and stir briefly with a graphite rod.
- Pour the melt into the preheated mold.
- Allow to cool, then remove the ingot.
- File a flat face and compare color and hardness (scratch test) with pure copper.
- Determine the density by water displacement and compare with the rule-of-mixtures estimate.
Observations & Expected Results
The ingot is golden-yellow, noticeably harder to file than pure copper, and its density falls between those of copper and zinc.
Worked Stoichiometric Calculations
Problem: Estimate the density of 70/30 brass by the rule of mixtures: 1/ρ = w(Cu)/ρ(Cu) + w(Zn)/ρ(Zn), with ρ(Cu) = 8.96 and ρ(Zn) = 7.14 g cm⁻³.
Working: 1/ρ = 0.70/8.96 + 0.30/7.14 = 0.07813 + 0.04202 = 0.12015, so ρ = 8.32 g cm⁻³ (typical measured values are 8.4-8.5).
Safety Precautions & Hazard Control
- Molten metal causes severe burns — full face shield, gloves, and closed shoes are mandatory.
- Zinc fumes are toxic; melt in a fume hood or well-ventilated area.
- Preheat the mold to avoid steam explosions from moisture.
- Keep water away from the molten metal.
Waste Disposal Protocol
Metal scrap and dross are collected for metal recycling; borax slag goes in general waste once cool.
Viva Voce Oral Defense Questions & Answers
Q: What is a substitutional solid solution?
A: An alloy in which solute atoms replace solvent atoms on the crystal lattice sites.
Q: Why is brass harder than pure copper?
A: Zinc atoms distort the lattice and pin dislocations, making slip harder.
Q: Why is flux used during melting?
A: To dissolve oxide films and protect the melt from air oxidation.