CHEMVEN

Seeded Growth of Cubic Crystals: Sodium Chloride from Brine

To grow cubic single crystals of sodium chloride on a seed and connect the cubic habit to the face-centered cubic lattice.

Level: UniversitySafety: SafeTime: 20 min setup + 4-6 days growth
Aim of Experiment: To grow cubic single crystals of sodium chloride on a seed and connect the cubic habit to the face-centered cubic lattice.

Theoretical Foundations

Sodium chloride crystallizes in the face-centered cubic (rock-salt) structure with a = 564 pm, so its natural growth form bounded by {100} faces is a cube. Adding a trace of urea or growing very slowly suppresses the usual hopper (skeletal) growth and gives solid cubes. This experiment links macroscopic crystal shape directly to the microscopic unit cell.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 250 mL beaker
  • Stirring rod
  • Filter funnel
  • Thread and stick
  • Seed crystal of NaCl
  • Magnifying lens

Chemical Reagents

  • Sodium chloride (about 60 g)
  • Distilled water (about 150 mL)
  • Urea (about 1 g, optional habit modifier)

Step-by-Step Practical Procedure

  1. Dissolve about 55 g of NaCl in 150 mL of warm distilled water and filter.
  2. Stir in about 1 g of urea to suppress hopper growth (optional).
  3. Suspend a small cubic seed crystal on a thread in the clear brine.
  4. Cover loosely and leave completely undisturbed at constant temperature.
  5. After 4-6 days of slow evaporation, remove the crystal.
  6. Rinse very briefly with ice-cold distilled water and blot dry immediately.
  7. Examine the faces with a magnifying lens.

Observations & Expected Results

Transparent to translucent cubes with flat {100} faces grow on the seed; without urea, hollow stepped 'hopper' cubes often form instead.

Worked Stoichiometric Calculations

Problem: NaCl has a = 564 pm, Z = 4, M = 58.44 g mol⁻¹. Calculate its theoretical density.

Working: ρ = ZM/(a³NA) = 4 × 58.44 / [(5.64 × 10⁻⁸ cm)³ × 6.022 × 10²³] = 233.76 / 108.0 = 2.16 g cm⁻³, matching the measured 2.165 g cm⁻³.

Safety Precautions & Hazard Control

  • Rinse only for a second; NaCl dissolves rapidly.
  • Keep dust out; each dust grain nucleates a competing crystal.
  • Do not use metal thread that could corrode in brine.
  • Handle the fragile cubes gently.

Waste Disposal Protocol

Brine may be poured down the drain with plenty of water.

Viva Voce Oral Defense Questions & Answers

Q: Why does NaCl naturally form cubes?

A: Its lattice is cubic (fcc rock-salt structure), and the slow-growing {100} faces bound the crystal as a cube.

Q: What are hopper crystals?

A: Skeletal cubes with hollow stepped faces, formed when edges grow faster than face centers at high supersaturation.

Q: How many formula units are in the NaCl unit cell?

A: Four (Z = 4).

← Back to Experiments Directory