Growing Piezoelectric Crystals: Rochelle Salt (Potassium Sodium Tartrate)
To grow large orthorhombic crystals of Rochelle salt and demonstrate their piezoelectric response.
Theoretical Foundations
Rochelle salt, potassium sodium tartrate tetrahydrate (KNaC4H4O6·4H2O), crystallizes in the orthorhombic system and is strongly piezoelectric: mechanical stress on the crystal generates an electric charge. It was the first material in which piezoelectricity was studied in detail and was used in early microphones and pickups. Slow evaporation of a saturated aqueous solution yields large, clear crystals.
Required Apparatus & Chemicals
Laboratory Apparatus
- 250 mL beaker
- Stirring rod
- Filter paper and funnel
- Thread and support
- Seed crystal
- Galvanometer or oscilloscope with leads
- Small hammer or clamp for stress test
Chemical Reagents
- Rochelle salt KNaC4H4O6·4H2O (about 70 g)
- Distilled water (about 150 mL)
- Aluminium foil (for piezo-test electrodes)
Step-by-Step Practical Procedure
- Dissolve about 65 g of Rochelle salt in 150 mL of warm distilled water (solubility is high, about 66 g per 100 mL at 20 °C).
- Filter into a clean beaker.
- Suspend a seed crystal on a thread in the solution.
- Cover loosely with filter paper and leave undisturbed for 7-10 days at constant temperature.
- Harvest a crystal of at least 2 cm and dry it gently.
- Attach thin foil electrodes or wires to opposite faces and connect to a galvanometer.
- Tap or squeeze the crystal gently and watch the galvanometer needle deflect.
Observations & Expected Results
Large, clear, orthorhombic crystals with a slightly wedge-shaped habit form; tapping the electroded crystal produces a visible galvanometer kick, proving piezoelectric charge generation.
Worked Stoichiometric Calculations
Problem: A Rochelle salt crystal of capacitance 50 pF develops 0.5 V when squeezed. Calculate the charge generated (Q = CV).
Working: Q = C × V = (50 × 10⁻¹² F) × 0.5 V = 25 × 10⁻¹² C = 25 pC. Even picocoulomb charges are detectable, showing the sensitivity of the piezoelectric effect.
Safety Precautions & Hazard Control
- Rochelle salt is non-toxic but keep crystals dry; they are slightly hygroscopic.
- Do not strike the crystal hard during the piezo test — it is brittle.
- Keep growth temperature steady; thermal cycling cracks the crystal.
- Wash hands after handling; the salt is a mild laxative if ingested.
Waste Disposal Protocol
Rochelle salt solutions are harmless and may be diluted and poured down the drain.
Viva Voce Oral Defense Questions & Answers
Q: What is the piezoelectric effect?
A: Mechanical stress on certain crystals generates an electric charge (and conversely, voltage causes strain).
Q: To which crystal system does Rochelle salt belong?
A: Orthorhombic.
Q: Name one historical application of Rochelle salt.
A: Early crystal microphones, phonograph pickups, and sonar transducers.