Available Alumina in Bauxite (Demo Leach)

To estimate caustic-soluble (available) alumina in bauxite by alkaline leaching.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To estimate caustic-soluble (available) alumina in bauxite by alkaline leaching.

Theoretical Foundations

In the Bayer process, gibbsite/boehmite dissolve in hot NaOH as sodium aluminate while iron and titanium stay insoluble (red mud). Leaching powdered bauxite with hot 10% NaOH, filtering, and precipitating aluminium as hydroxide (or titrating the aluminate) estimates the economically available alumina, distinct from total alumina locked in clays.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Round-bottom flask with condenser
  • Water bath
  • Buchner funnel
  • Balance
  • pH paper

Chemical Reagents

  • Bauxite powder (5 g)
  • Sodium hydroxide solution (10%, 100 mL)
  • Dilute HCl
  • Ammonia solution

Step-by-Step Practical Procedure

  1. Digest 5 g bauxite with 100 mL hot 10% NaOH under reflux for 1 hour.
  2. Filter hot and wash the red mud residue with hot water.
  3. Acidify the filtrate, then precipitate aluminium hydroxide with ammonia at pH 7.
  4. Filter, wash, ignite at 1000 C and weigh as Al2O3.
  5. Calculate available alumina % on the bauxite weight.

Observations & Expected Results

Good bauxite yields 40-55% available alumina as white ignited residue; the red mud stays brick-red.

Worked Stoichiometric Calculations

Problem: 5.0 g bauxite gave 2.35 g ignited Al2O3. Calculate the available alumina percentage.

Working: Available alumina = 2.35/5.0 x 100 = 47%, a good metallurgical-grade bauxite.

Safety Precautions & Hazard Control

  • Hot NaOH is caustic; wear gloves and goggles.
  • Filter hot; aluminate crystallises on cooling.
  • Wash the precipitate free of sodium.
  • Ignite to constant weight.

Waste Disposal Protocol

Red mud goes to solid waste; alkaline filtrates are neutralised first.

Viva Voce Oral Defense Questions & Answers

Q: What is red mud?

A: The insoluble residue of bauxite digestion: mainly iron oxide, titanium dioxide and silica compounds.

Q: Why is only 'available' alumina counted?

A: Alumina bound in kaolinite clay does not dissolve in the Bayer digest and cannot be recovered economically.