Zinc Coating Thickness on Galvanised Steel
To determine the zinc coating mass on galvanised steel by the strip-and-weigh method.
Theoretical Foundations
The zinc layer is dissolved in inhibited hydrochloric acid (with antimony chloride to protect the steel), and the mass loss gives the coating mass per unit area. Dividing by zinc's density (7.14 g/cc) gives the average thickness. The result is expressed as g/m2, the commercial specification unit (e.g. Z275 = 275 g/m2 total both sides).
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- Vernier caliper
- Beaker
- Tongs
Chemical Reagents
- Galvanised steel coupon (known area)
- Hydrochloric acid with antimony chloride inhibitor
Step-by-Step Practical Procedure
- Measure the coupon dimensions and calculate total surface area (both sides).
- Weigh the coupon (W1).
- Immerse in the inhibited acid until hydrogen evolution stops (zinc dissolved).
- Rinse, dry and weigh (W2).
- Calculate coating mass = (W1 - W2)/area in g/m2 and thickness = mass/density.
- Compare with the specified coating class.
Observations & Expected Results
Hydrogen bubbles vigorously then stops when zinc is gone, leaving a grey steel surface; typical coatings are 100-300 g/m2.
Worked Stoichiometric Calculations
Problem: A 10 cm x 10 cm coupon (both sides = 0.02 m2) lost 4.4 g. Calculate the coating mass in g/m2 and the thickness in microns.
Working: Coating = 4.4/0.02 = 220 g/m2. Thickness = 220 g/m2 / 7.14 g/cc = 30.8 cc/m2 = 30.8 microns.
Safety Precautions & Hazard Control
- Use inhibited acid; uninhibited acid attacks the steel and inflates the loss.
- Stop promptly when bubbling ceases.
- Dry completely before the final weighing.
- Handle HCl with gloves and goggles.
Waste Disposal Protocol
Zinc-containing acid goes to heavy-metal waste after neutralisation.
Viva Voce Oral Defense Questions & Answers
Q: How does galvanising protect steel?
A: Zinc corrodes preferentially (sacrificial protection) and its corrosion products form a barrier film over the steel.
Q: What is Z275?
A: A coating class meaning 275 g of zinc per square metre total on both sides.