CHEMVEN

Iron in Iron Ore by Dichromate Titration

To determine total iron in haematite ore by stannous chloride reduction and dichromate titration.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: To determine total iron in haematite ore by stannous chloride reduction and dichromate titration.

Theoretical Foundations

The ore is dissolved in HCl, oxidising iron to Fe3+. Stannous chloride reduces Fe3+ to Fe2+ (end point: disappearance of yellow), excess SnCl2 is destroyed with HgCl2 (silky white Hg2Cl2 confirms slight excess), and Fe2+ is titrated with standard K2Cr2O7 using diphenylamine indicator. 1 mL of 0.1 N dichromate = 5.585 mg Fe.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Conical flasks
  • Burette
  • Pipette
  • Hot plate

Chemical Reagents

  • Iron ore (0.5 g, powdered)
  • Concentrated HCl
  • Stannous chloride solution
  • Mercuric chloride solution
  • 0.1 N potassium dichromate (standardised)
  • Diphenylamine indicator
  • Phosphoric-sulphuric acid mixture

Step-by-Step Practical Procedure

  1. Dissolve 0.5 g ore in 20 mL concentrated HCl with heating; filter off silica.
  2. Dilute, heat to boiling, and add SnCl2 dropwise until the yellow Fe3+ colour just disappears, plus 2 drops excess.
  3. Cool rapidly and add HgCl2 solution; a silky white precipitate should form.
  4. Add the acid mixture and diphenylamine indicator.
  5. Titrate with 0.1 N K2Cr2O7 to the violet-blue end point.
  6. Calculate Fe % = titre x 0.005585 x 100 / ore weight.

Observations & Expected Results

Haematite gives titres corresponding to 55-65% Fe; the white Hg2Cl2 precipitate confirms correct reduction.

Worked Stoichiometric Calculations

Problem: 0.500 g ore required 58.5 mL of 0.1 N K2Cr2O7. Calculate the iron percentage.

Working: Fe = 58.5 x 0.005585 x 100/0.500 = 32.67/0.500 = 65.3% Fe, a rich haematite ore.

Safety Precautions & Hazard Control

  • Add only slight excess SnCl2; large excess gives grey mercury metal and low results.
  • Cool before adding HgCl2.
  • Titrate promptly after reduction; air re-oxidises Fe2+.
  • Mercuric chloride is toxic; handle with gloves.

Waste Disposal Protocol

Mercury-containing residues go to the toxic heavy-metal waste container.

Viva Voce Oral Defense Questions & Answers

Q: Why is HgCl2 added?

A: It destroys excess SnCl2 as white Hg2Cl2; without this, leftover SnCl2 would consume dichromate and inflate the iron result.

Q: Why add phosphoric acid?

A: It complexes Fe3+ as colourless Fe(HPO4)+, removing the yellow colour so the diphenylamine end point is visible.

← Back to Experiments Directory