Corrosion Rate by Weight Loss (Coupons)

To determine the corrosion rate of mild steel in acid and salt media by weight loss.

Level: UniversitySafety: Needs supervisionTime: 7 days (exposure)
Aim of Experiment: To determine the corrosion rate of mild steel in acid and salt media by weight loss.

Theoretical Foundations

Clean, weighed steel coupons are immersed in corrosive media for a fixed time; the mass loss gives the average corrosion rate: mpy = (534 x loss in mg) / (density x area in sq.in x time in hours). Comparing media and inhibitor doses quantifies corrosivity and inhibitor efficiency, the basis of materials selection.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Glass jars
  • Analytical balance
  • Vernier caliper
  • Steel coupons
  • Water bath (optional)

Chemical Reagents

  • 1 N hydrochloric acid
  • 3.5% sodium chloride solution
  • Corrosion inhibitor (e.g. sodium nitrite)
  • Acetone
  • Inhibited cleaning acid

Step-by-Step Practical Procedure

  1. Degrease coupons with acetone, dry, weigh (W1), and measure dimensions.
  2. Immerse triplicate coupons in each medium: HCl, salt water, salt water + inhibitor.
  3. Keep 7 days at room temperature, topping up evaporation.
  4. Remove, clean off corrosion products in inhibited acid, rinse, dry and weigh (W2).
  5. Calculate mpy for each medium and inhibitor efficiency % = (uninhibited - inhibited) x 100 / uninhibited.

Observations & Expected Results

Steel in 1 N HCl loses visibly with hydrogen bubbling (hundreds of mpy); in salt water it rusts brown (tens of mpy); inhibitor cuts the loss sharply.

Worked Stoichiometric Calculations

Problem: A coupon (area 5 sq.in, density 7.86 g/cc) lost 250 mg in 168 hours. Calculate the corrosion rate in mpy.

Working: mpy = 534 x 250/(7.86 x 5 x 168) = 133500/6602.4 = 20.2 mpy, a moderate rate for salt water.

Safety Precautions & Hazard Control

  • Weigh coupons to 0.1 mg; small errors dominate.
  • Clean corrosion products without attacking base metal (use inhibited acid).
  • Keep immersion times identical.
  • Handle HCl with gloves and goggles.

Waste Disposal Protocol

Acid media are neutralised before disposal; coupons go to metal waste.

Viva Voce Oral Defense Questions & Answers

Q: What is mpy?

A: Mils per year: thousandths of an inch of metal lost per year, the standard engineering corrosion rate unit.

Q: How do inhibitors work?

A: They adsorb on the metal surface, blocking anodic or cathodic sites and slowing the electrochemical corrosion reactions.