Sizing Test of Paper (Ink Flotation)
To test the sizing (water resistance) of paper samples.
Theoretical Foundations
Sizing agents (rosin-alum or AKD) make paper resist water and ink penetration so writing does not feather. In the ink flotation test, paper boats float on ink; the time for ink to penetrate and show through measures sizing degree. Well-sized writing paper resists for minutes; blotting paper fails in seconds.
Required Apparatus & Chemicals
Laboratory Apparatus
- Petri dishes
- Stopwatch
- Scissors
Chemical Reagents
- Paper samples (writing, newsprint, blotting)
- Fountain pen ink (diluted)
Step-by-Step Practical Procedure
- Cut identical paper boats or strips from each sample.
- Pour diluted ink into petri dishes.
- Float one boat per dish simultaneously and start the stopwatch.
- Record the time when ink first shows through on the upper surface.
- Rank the papers by penetration time.
- Optionally test both sides of each paper.
Observations & Expected Results
Blotting paper fails in under 10 seconds; good writing paper resists 2-5 minutes; newsprint is intermediate.
Worked Stoichiometric Calculations
Problem: Writing paper resisted 180 s, newsprint 45 s, blotting paper 8 s. Express each as a multiple of the blotting paper time.
Working: Writing: 180/8 = 22.5x; newsprint: 45/8 = 5.6x; blotting: 1x. Writing paper is about 22 times better sized.
Safety Precautions & Hazard Control
- Cut samples to identical size.
- Start all boats at the same moment.
- Keep the ink depth the same in each dish.
- Handle papers by the edges; finger grease affects sizing.
Waste Disposal Protocol
Ink-stained papers go to solid waste; ink goes to chemical waste.
Viva Voce Oral Defense Questions & Answers
Q: What is rosin sizing?
A: Rosin soap precipitated with alum onto fibres makes paper water-repellent; it is the traditional acid sizing system.
Q: Why is blotting paper unsized?
A: It is meant to absorb ink instantly, so sizing agents are deliberately omitted.