Wash Fastness of Dyed Fabric

To assess the wash fastness of dyed fabrics using a standard soap test.

Level: UniversitySafety: SafeTime: 60 min
Aim of Experiment: To assess the wash fastness of dyed fabrics using a standard soap test.

Theoretical Foundations

Wash fastness measures how well a dye resists bleeding and fading during laundering. The dyed sample stitched to white cotton is agitated in soap solution at 60 C; afterwards the colour change of the dyed piece and the staining of the white piece are graded against grey scales from 5 (excellent) to 1 (poor). Reactive dyes score 4-5, direct dyes 2-4.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Water bath with shaker
  • Beakers
  • Grey scales for colour change and staining
  • Needle and thread

Chemical Reagents

  • Dyed fabric samples
  • White cotton adjacent fabric
  • Soap solution (5 g/L)
  • Sodium carbonate (2 g/L)

Step-by-Step Practical Procedure

  1. Stitch each dyed sample to a piece of white cotton.
  2. Prepare the soap-soda wash liquor at 60 C.
  3. Agitate the composites in the liquor for 30 minutes.
  4. Rinse in cold water and dry.
  5. Grade colour change of the dyed fabric against the grey scale.
  6. Grade staining of the white fabric against the staining scale.
  7. Rank the dyes by fastness.

Observations & Expected Results

Reactive-dyed cotton keeps grade 4-5 with negligible staining; direct-dyed cotton fades to grade 3 and stains the white.

Worked Stoichiometric Calculations

Problem: A dye scores colour-change grade 4 and staining grade 3-4. A second scores 3 and 2. Which has better wash fastness overall?

Working: The first dye is better on both measures: less fading (4 vs 3) and less staining (3-4 vs 2).

Safety Precautions & Hazard Control

  • Keep temperature and time identical for all samples.
  • Use the standard liquor ratio for comparability.
  • Dry samples away from direct sunlight before grading.
  • Grade in standard daylight, not yellow lamplight.

Waste Disposal Protocol

Wash liquors go to chemical waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the difference between the two grey scales?

A: One grades fading of the dyed sample; the other grades staining transferred to the adjacent white fabric.

Q: Why do reactive dyes have the best wash fastness?

A: They form covalent bonds with cellulose, so the dye cannot desorb during washing.