CHEMVEN

Direct Dyeing of Cotton

To dye cotton with a direct dye and study the effect of salt.

Level: UniversitySafety: SafeTime: 60 min
Aim of Experiment: To dye cotton with a direct dye and study the effect of salt.

Theoretical Foundations

Direct dyes are large planar anionic molecules that hydrogen-bond to cellulose and are held by van der Waals forces. Common salt (NaCl) suppresses the fibre's negative surface charge, driving dye exhaustion from bath to fabric. The experiment compares dye uptake with and without salt.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • Water bath
  • Glass rods
  • Weighing balance

Chemical Reagents

  • Cotton fabric pieces (5 g each)
  • Direct dye e.g. Congo red (2% owf)
  • Sodium chloride (10 g/L)
  • Detergent for scouring

Step-by-Step Practical Procedure

  1. Scour the cotton by boiling with detergent, rinse and dry.
  2. Prepare two dye baths (2% dye on weight of fabric) at 90 C; add 10 g/L salt to one only.
  3. Enter the wetted fabrics and dye for 45 minutes with occasional stirring.
  4. Remove, rinse cold, and dry.
  5. Compare the depth of shade visually or with a colorimeter.
  6. Test wash fastness of each with soap solution at 60 C.

Observations & Expected Results

The salt bath gives a markedly deeper shade; without salt the fabric dyes pale and uneven.

Worked Stoichiometric Calculations

Problem: 5 g fabric dyed at 2% owf needs how much dye? If the salt bath exhausts 90% and the no-salt bath 50%, how much dye fixes on each?

Working: Dye used = 0.02 x 5 = 0.10 g. Salt bath fixes 0.09 g; no-salt bath fixes 0.05 g, i.e. 80% more dye with salt.

Safety Precautions & Hazard Control

  • Scour the fabric or dyeing is patchy.
  • Maintain 90 C for level dyeing.
  • Stir gently to avoid felting.
  • Wear gloves; direct dyes stain skin.

Waste Disposal Protocol

Spent dye baths go to chemical waste, not the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why does salt help direct dyeing?

A: It shields the electrostatic repulsion between the anionic dye and the negatively charged cotton surface, letting dye molecules approach and adsorb.

Q: What is 'owf'?

A: 'On weight of fabric': dye percentages are quoted relative to the dry fabric weight.

← Back to Experiments Directory