Novolac vs Resol: Two Phenolic Resins
To prepare novolac and resol resins and compare their curing behaviour.
Theoretical Foundations
Acid catalysis with excess phenol gives novolac: linear chains that stay fusible until a hardener (hexamine) is added. Alkaline catalysis with excess formaldehyde gives resol: methylol-rich chains that crosslink on heating alone. Comparing them shows how catalyst and ratio decide whether a resin is a thermoplastic intermediate or a self-curing thermoset.
Required Apparatus & Chemicals
Laboratory Apparatus
- Two round-bottom flasks
- Reflux condensers
- Water baths
- Moulds
- Oven
Chemical Reagents
- Phenol
- Formalin
- Concentrated HCl (for novolac)
- Sodium hydroxide (for resol)
- Hexamine (for novolac cure)
Step-by-Step Practical Procedure
- Novolac: reflux phenol with formalin (molar ratio 1:0.8) and HCl catalyst for 1 hour; separate the resin.
- Resol: warm phenol with formalin (ratio 1:1.5) and NaOH at 60 C for 1 hour.
- Try melting a sample of each on a hot plate: novolac softens, resol begins to harden.
- Mix hexamine into the novolac, mould both, and cure at 150 C.
- Compare hardness, colour and infusibility of the cured products.
Observations & Expected Results
Novolac is a brittle amber solid needing hexamine to cure; resol is a syrup that hardens on heating alone.
Worked Stoichiometric Calculations
Problem: For novolac, 9.4 g phenol (0.1 mol) needs 0.08 mol formaldehyde. What volume of 37% formalin (density 1.09, 13.6 M) is required?
Working: Volume = 0.08/13.6 = 0.00588 L = 5.9 mL of formalin.
Safety Precautions & Hazard Control
- Phenol is corrosive; wear gloves and goggles.
- Work in a fume cupboard because of formalin.
- Control exotherms during reflux.
- Handle hot moulds with gloves.
Waste Disposal Protocol
Aqueous layers go to chemical waste; cured resins are solid waste.
Viva Voce Oral Defense Questions & Answers
Q: Why does novolac need hexamine?
A: Its linear chains lack reactive methylol groups; hexamine supplies the methylene bridges for crosslinking on heating.
Q: Which type is used in grinding wheels?
A: Resol-type resins, often as the bond for abrasive wheels because they cure hard and heat-resistant.