Crosslinking Demo: PVA-Borax Gel

To demonstrate polymer crosslinking by forming a PVA-borax gel.

Level: UniversitySafety: SafeTime: 30 min
Aim of Experiment: To demonstrate polymer crosslinking by forming a PVA-borax gel.

Theoretical Foundations

Polyvinyl alcohol chains are linked by borate ions, which complex with adjacent hydroxyl groups to form reversible crosslinks. The solution transforms into a viscoelastic gel (slime): it flows slowly like a liquid but bounces and snaps like a solid, a vivid model of crosslinked polymer behaviour.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • Glass rods
  • Measuring cylinders

Chemical Reagents

  • Polyvinyl alcohol solution (4%, 100 mL)
  • Borax solution (4%, 10 mL)
  • Food colour (optional)

Step-by-Step Practical Procedure

  1. Pour 100 mL PVA solution into a beaker and stir in food colour.
  2. Add 10 mL borax solution while stirring vigorously.
  3. Observe the sudden gelation within seconds.
  4. Knead the gel and test: stretch slowly (flows), pull fast (snaps), roll into a ball (bounces).
  5. Repeat with half the borax and compare stiffness.
  6. Record how crosslinker amount changes the gel properties.

Observations & Expected Results

The liquid sets into a clear, stretchy slime; more borax gives a firmer, less stretchy gel.

Worked Stoichiometric Calculations

Problem: 100 mL of 4% PVA contains 4 g polymer. If 10 mL of 4% borax (0.4 g) is added, what is the borax-to-polymer mass ratio?

Working: 0.4/4.0 = 0.10, i.e. a 10% crosslinker ratio by mass.

Safety Precautions & Hazard Control

  • Borax is mildly toxic; do not ingest and wash hands after.
  • Keep slime away from fabrics and hair.
  • Use clean glassware; impurities affect gelation.
  • Dispose, do not pour large gels down the drain.

Waste Disposal Protocol

Collect the gel in solid waste; rinse small residues down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Are the borate crosslinks permanent?

A: No, they are reversible hydrogen-bonded complexes, which is why the slime flows slowly and can be re-kneaded.

Q: What is the industrial use of this chemistry?

A: Borate crosslinking thickens fluids in cosmetics, adhesives and oilfield fracturing fluids.