CHEMVEN

Proximate Analysis of Coal: Ash Content

To determine the ash content of coal (proximate analysis, part 3).

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine the ash content of coal (proximate analysis, part 3).

Theoretical Foundations

Ash is the incombustible mineral residue left after burning coal at 815 C to constant weight. It comes from clay, shale and pyrite in the coal. High ash lowers the calorific value, causes slagging in furnaces and increases handling costs; power-station coal is typically limited to about 34% ash.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Muffle furnace (815 C)
  • Silica dish
  • Tongs
  • Desiccator
  • Analytical balance

Chemical Reagents

  • Coal sample (1 g, 72-mesh)

Step-by-Step Practical Procedure

  1. Weigh 1 g coal into a tared silica dish.
  2. Heat in the furnace, raising to 815 C, and ignite to constant weight (about 1-2 hours).
  3. Stir once midway to expose unburnt carbon.
  4. Cool in a desiccator and weigh.
  5. Calculate ash % = residue x 100 / sample weight.

Observations & Expected Results

Good steam coal leaves 10-20% grey-red ash; high-ash coals leave over 35% and burn poorly.

Worked Stoichiometric Calculations

Problem: 1.000 g coal left 0.185 g ash. A power plant rejects coal above 34% ash. Calculate and judge.

Working: Ash = 18.5%, well below the 34% rejection limit: acceptable for the power plant.

Safety Precautions & Hazard Control

  • Ignite to constant weight; trapped carbon inflates nothing but underestimates ash.
  • Do not exceed 815 C; some ash constituents volatilise at higher temperatures.
  • Cool in a desiccator before weighing.
  • Handle hot dishes with tongs only.

Waste Disposal Protocol

Ash goes to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Is ash originally present in coal?

A: Mostly yes as mineral matter (inherent ash), plus some picked up during mining (adventitious ash).

Q: Why is ash a problem in boilers?

A: It forms slag and clinker on tubes, erodes equipment and must be collected and disposed of.

← Back to Experiments Directory