CHEMVEN

Compressive Strength of Cement Mortar Cubes

To determine the compressive strength of 1:3 cement mortar cubes at 3 and 7 days.

Level: UniversitySafety: Needs supervisionTime: 3 days (with curing)
Aim of Experiment: To determine the compressive strength of 1:3 cement mortar cubes at 3 and 7 days.

Theoretical Foundations

Compressive strength is the defining performance grade of cement (e.g. 43 grade means at least 43 MPa at 28 days). Standard 70.6 mm cubes of 1:3 cement-sand mortar with (P/4 + 3)% water are cured in water and crushed in a compression testing machine; strength = failure load / cross-sectional area (5000 mm2).

Required Apparatus & Chemicals

Laboratory Apparatus

  • Cube moulds (70.6 mm)
  • Compression testing machine
  • Curing tank
  • Tamping rod
  • Balance

Chemical Reagents

  • Cement
  • Standard Ennore sand
  • Distilled water

Step-by-Step Practical Procedure

  1. Mix 1 part cement with 3 parts standard sand and (P/4 + 3)% water to a uniform mortar.
  2. Fill cube moulds in layers, tamping each layer 25 times.
  3. Keep 24 hours in moist air, demould, and cure in clean water.
  4. Crush three cubes at 3 days and three at 7 days in the compression machine at a steady loading rate.
  5. Calculate strength = load (N) / 5000 mm2 and average each age group.

Observations & Expected Results

43-grade OPC gives about 23 MPa at 3 days and 33 MPa at 7 days; failure shows a characteristic double-pyramid fracture.

Worked Stoichiometric Calculations

Problem: A cube failed at 165 kN at 7 days. Calculate the compressive strength in MPa.

Working: Strength = 165000 N / 5000 mm2 = 33 MPa. This meets the typical 7-day expectation for 43-grade cement.

Safety Precautions & Hazard Control

  • Use standard graded sand; ordinary sand gives erratic results.
  • Tamp uniformly to avoid honeycombing.
  • Keep curing water clean and at 27 C.
  • Apply load at the specified rate; shock loading lowers the reading.

Waste Disposal Protocol

Crushed cubes go to solid construction waste.

Viva Voce Oral Defense Questions & Answers

Q: Why 70.6 mm cubes?

A: The face area is exactly 50 cm2 (5000 mm2), simplifying the stress calculation.

Q: Why is sand limited to 3 parts?

A: The 1:3 ratio is the standard that defines cement grades, keeping results comparable worldwide.

← Back to Experiments Directory