CHEMVEN

Plastic Waste Identification: Density and Beilstein Tests

To identify common plastics in waste by density separation and the Beilstein test.

Level: UniversitySafety: Needs supervisionTime: 60 min
Aim of Experiment: To identify common plastics in waste by density separation and the Beilstein test.

Theoretical Foundations

Plastics have characteristic densities (PE/PP <1 float in water; PS ~1.05; PET ~1.38, PVC ~1.4 sink in water but separate in salt solutions) and the Beilstein test (green copper-halide flame) detects PVC's chlorine. Identification enables proper recycling segregation; PVC contaminates PET recycling and releases dioxins if burnt.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Beakers
  • Copper wire
  • Bunsen burner
  • Balance
  • Water/ethanol/salt solutions

Chemical Reagents

  • Sodium chloride solutions (various densities)
  • Ethanol
  • Distilled water

Step-by-Step Practical Procedure

  1. Cut small pieces of each unknown plastic.
  2. Drop into water: floaters are PE/PP.
  3. Test sinkers in salt solutions of increasing density to separate PS, PET, PVC.
  4. Heat a copper wire, touch the plastic, and burn: green flame = PVC (Beilstein positive).
  5. Confirm PE vs PP by further density/ethanol tests.
  6. Tabulate identifications and recommend recycling streams.

Observations & Expected Results

PE/PP float; PET sinks in water; PVC gives a green Beilstein flame.

Worked Stoichiometric Calculations

Problem: A 2.0 cm3 plastic piece weighs 2.76 g. Calculate density and identify the likely plastic.

Working: Density = 2.76/2.0 = 1.38 g/cm3 - matches PET (1.38); confirm with a sink-in-water test and check it is not PVC via Beilstein.

Safety Precautions & Hazard Control

  • Burn only tiny pieces; fumes are toxic (especially PVC).
  • Work in a ventilated area.
  • Handle the hot copper wire with tongs.
  • Do not inhale burning-plastic fumes.

Waste Disposal Protocol

Test pieces to plastic recycling or solid waste.

Viva Voce Oral Defense Questions & Answers

Q: What is the chemistry of the Beilstein test?

A: Heated copper reacts with organic halides to form volatile copper halides that colour the flame green.

Q: Why must PVC be kept out of PET recycling?

A: PVC degrades at PET processing temperatures, discolouring and weakening the recycled product.

Q: Why do PE and PP float in water?

A: Their densities (0.90-0.96 g/cm3) are below water's 1.0 g/cm3.

← Back to Experiments Directory