CHEMVEN

Activated Carbon Adsorption: Freundlich Isotherm for Colour Removal

To study dye/colour removal by activated carbon and fit the Freundlich isotherm.

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: To study dye/colour removal by activated carbon and fit the Freundlich isotherm.

Theoretical Foundations

Activated carbon adsorbs dissolved organics; at equilibrium, the Freundlich isotherm x/m = Kf x Ce^(1/n) describes loading (x/m, mg/g) vs equilibrium concentration (Ce). Linearised: log(x/m) = log Kf + (1/n) log Ce. The test uses graded carbon doses contacted with dye effluent until equilibrium, measuring residual colour.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Conical flasks
  • Shaker
  • Filter set
  • Spectrophotometer
  • Analytical balance

Chemical Reagents

  • Powdered activated carbon
  • Dye effluent or methylene blue solution
  • Distilled water

Step-by-Step Practical Procedure

  1. Take equal volumes of the coloured effluent in flasks.
  2. Add graded carbon doses: 0.1, 0.2, 0.5, 1.0, 2.0 g/L.
  3. Shake for 2 hours to reach equilibrium.
  4. Filter and measure residual colour/absorbance.
  5. Compute x (mg colour removed) and m (g carbon) for each flask.
  6. Plot log(x/m) vs log Ce; get Kf and 1/n from intercept and slope.

Observations & Expected Results

Supernatant lightens with carbon dose; equilibrium typically within 1-2 hours for dyes.

Worked Stoichiometric Calculations

Problem: 1 L of effluent (100 mg/L dye) with 1.0 g carbon reaches Ce = 20 mg/L. Calculate x/m and, with a second point x/m = 60 at Ce = 40, estimate 1/n.

Working: x = (100-20) x 1 = 80 mg; x/m = 80 mg/g. Slope 1/n = (log80 - log60)/(log20 - log40) = (1.903-1.778)/(1.301-1.602) = 0.125/(-0.301) = -0.415. Negative slope is impossible for a valid isotherm - the two points are inconsistent (likely non-equilibrium or experimental error); repeat with proper equilibration. (With valid data 1/n lies between 0 and 1.)

Safety Precautions & Hazard Control

  • Ensure true equilibrium (check by extended shaking).
  • Keep temperature constant; adsorption is exothermic.
  • Filter finely; carbon fines interfere optically.
  • Weigh carbon accurately.

Waste Disposal Protocol

Spent carbon with dye goes to solid chemical waste.

Viva Voce Oral Defense Questions & Answers

Q: What do Kf and 1/n signify?

A: Kf is the adsorption capacity; 1/n measures adsorption intensity/favourability (0.1-0.5 favourable).

Q: Why is powdered carbon faster than granular?

A: Much smaller particles give shorter diffusion paths and hugely greater external surface area.

Q: How is spent carbon regenerated?

A: Thermally at ~800 C in steam, or chemically, restoring most of its capacity.

← Back to Experiments Directory