Nickel in Alloy: EDTA with Murexide

To determine % Ni in a nickel alloy by EDTA titration.

Level: UniversitySafety: Needs supervisionTime: 75 min
Aim of Experiment: To determine % Ni in a nickel alloy by EDTA titration.

Theoretical Foundations

Ni2+ + H2Y(2-) -> NiY(2-) + 2H+ at pH 10 (log K = 18.6). Murexide forms a yellow complex with Ni2+; the endpoint is yellow to violet. The solution is heated slightly because Ni-EDTA formation can be slow in the cold.

Required Apparatus & Chemicals

Laboratory Apparatus

  • 50 mL burette
  • 25 mL pipette
  • 250 mL volumetric flask
  • 250 mL conical flask
  • Analytical balance
  • Bunsen burner

Chemical Reagents

  • Nickel alloy sample
  • Dilute HNO3
  • Standardised EDTA (0.01004 M)
  • pH 10 buffer
  • Murexide indicator

Step-by-Step Practical Procedure

  1. Weigh about 0.5000 g alloy; dissolve in dilute HNO3; make up to 250.0 mL.
  2. Pipette 25.00 mL into a flask; add pH 10 buffer.
  3. Add murexide (yellow).
  4. Warm to about 40 C.
  5. Titrate with 0.01004 M EDTA to the violet endpoint.
  6. Calculate % Ni (M = 58.69).

Observations & Expected Results

Yellow to violet endpoint. Typical titre about 12.80 mL.

Worked Stoichiometric Calculations

Problem: 0.5000 g alloy to 250.0 mL; 25.00 mL aliquot needed 12.80 mL of 0.01004 M EDTA. Find % Ni.

Working: Moles EDTA = 0.01004 x 0.01280 = 0.00012851 mol = moles Ni2+ in aliquot. In 250 mL: 0.0012851 mol. Mass = 0.0012851 x 58.69 = 0.075423 g. % = 0.075423/0.5000 x 100 = 15.1%.

Safety Precautions & Hazard Control

  • Warm the solution; cold Ni2+ reacts sluggishly with EDTA.
  • Keep pH at 10; Ni(OH)2 precipitates above 11.
  • Dissolve alloy in a fume cupboard.

Waste Disposal Protocol

Nickel waste to heavy-metal aqueous waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the titration warmed?

A: Ni2+ is kinetically inert (slow ligand exchange); warming speeds complex formation so the endpoint is sharp.

Q: Which other ions interfere?

A: Cu2+, Co2+ and Fe3+ also complex EDTA and murexide; they must be masked or separated.