Theoretical Foundations

Each polymer has marker bands: PE: 2920/2850 (C−H), 1465, 720 cm⁻¹; PS: 3025, 1600, 700 cm⁻¹ (aromatic); PVC: 615 cm⁻¹ (C−Cl); PET: 1720 (ester C=O), 1250 cm⁻¹. Thin films or ATR spectra matched against these markers identify the plastic.

Required Apparatus & Chemicals

Laboratory Apparatus

  • FTIR spectrometer (ATR preferred)
  • Scissors
  • Unknown plastic pieces
  • Tweezers
  • Ethanol wipes (crystal cleaning)

Chemical Reagents

  • PE reference (plastic bag piece)
  • PS reference (cup piece)
  • PVC reference (pipe piece)
  • PET reference (bottle piece)
  • Ethanol (for cleaning ATR crystal)

Step-by-Step Practical Procedure

  1. Record ATR spectra of the four reference plastics.
  2. Tabulate each polymer's 2-3 marker bands.
  3. Record spectra of 3 unknown pieces.
  4. Match marker bands to identify each.
  5. Confirm with a second band per polymer.
  6. Report the identifications with evidence.

Observations & Expected Results

PE shows the 720 cm⁻¹ rocking band; PS the 700 cm⁻¹ aromatic band; PVC the strong 615 cm⁻¹ C−Cl; PET the 1720 cm⁻¹ ester carbonyl.

Worked Stoichiometric Calculations

Problem: An unknown shows strong bands at 1720 and 1250 cm⁻¹ but none at 615 cm⁻¹. Identify it.

Working: 1720 cm⁻¹ (ester C=O) + 1250 cm⁻¹ (C−O) = PET polyester; absence of 615 cm⁻¹ rules out PVC.

Safety Precautions & Hazard Control

  • Clean the ATR crystal between samples.
  • Ensure good sample-crystal contact.
  • Cut samples to fit the crystal.
  • Compare with references run the same day.

Waste Disposal Protocol

Plastic pieces to recycling/solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is the 720 cm⁻¹ band diagnostic for PE?

A: It is the CH2 rocking mode of long polymethylene chains, characteristic of polyethylene.

Q: How do PS and PET differ spectroscopically?

A: PS has aromatic C−H/C=C bands without carbonyl; PET has the strong ester C=O at 1720 cm⁻¹.

Q: Why is ATR convenient for plastics?

A: No sample preparation: the piece is simply pressed on the crystal, ideal for solid polymers.