Flame AAS: Copper in Brass at 324.8 nm
To determine % copper in brass by flame atomic absorption at 324.8 nm.
Theoretical Foundations
In AAS, ground-state Cu atoms in an air-acetylene flame absorb the 324.8 nm line from a copper hollow-cathode lamp. Absorbance is proportional to Cu concentration (Beer's law for atoms). AAS is more specific than flame emission because the line source isolates the analyte wavelength.
Required Apparatus & Chemicals
Laboratory Apparatus
- Atomic absorption spectrometer
- Cu hollow-cathode lamp
- Air-acetylene burner
- Volumetric flasks
- Pipettes
Chemical Reagents
- Brass (0.100 g)
- Nitric acid (conc.)
- Cu standard (100 mg L⁻¹)
- Distilled water
Step-by-Step Practical Procedure
- Dissolve 0.100 g brass in conc. HNO3 in a fume cupboard; dilute to 100 mL.
- Dilute 1.00 mL to 100 mL.
- Prepare Cu standards 0-10 mg L⁻¹ in dilute HNO3.
- Install the Cu lamp; optimize the 324.8 nm line and flame.
- Zero with the acid blank; read standards.
- Read the sample; calculate % Cu.
Observations & Expected Results
Absorbance linear with Cu; typical slope ≈ 0.15 A·L mg⁻¹; Zn causes no spectral interference at 324.8 nm.
Worked Stoichiometric Calculations
Problem: Slope 0.15 A·L mg⁻¹. 0.100 g brass to 100 mL; 1.00 mL diluted to 100 mL gives A = 0.975. Find % Cu.
Working: c(measured) = 0.975/0.15 = 6.50 mg L⁻¹. Stock = 650 mg L⁻¹. In 0.100 L: 65.0 mg Cu. %Cu = 65.0/100 × 100 = 65.0%.
Safety Precautions & Hazard Control
- Acetylene is explosive: leak-check, flashback arrestors, trained supervision.
- Never look directly at the hollow-cathode beam.
- Matrix-match standards in dilute HNO3.
- Allow lamp warm-up for stable output.
Waste Disposal Protocol
Acidic Cu/Zn waste to the aqueous heavy-metal waste bottle.
Viva Voce Oral Defense Questions & Answers
Q: Why is AAS more specific than flame photometry?
A: The hollow-cathode lamp emits only the sharp analyte line, so only ground-state analyte atoms absorb; other elements cannot contribute.
Q: Why use an air-acetylene flame?
A: It is hot enough (~2300 °C) to atomize copper efficiently while keeping ionization low.
Q: What is the role of the hollow-cathode lamp?
A: It provides the intense, narrow resonance line that the analyte atoms absorb.